16Mo3 Pipe Supplier in Mumbai, India

ALLOY STEEL PIPE
Metals Fabrica supplies 16Mo3 (1.5415) seamless molybdenum steel pipe and tube to EN 10216-2 for boiler, header and pressure piping at elevated temperature, with matching EN 10028-2 plate.
Steel pipes and tubes in bundles on racks in an industrial warehouse
OVERVIEW

16Mo3 Pipe Overview

16Mo3 (material number 1.5415) is a European non-alloy-plus-molybdenum steel for pressure purposes at elevated temperature. Its 0.25–0.35% molybdenum improves creep and tensile strength at temperature compared with carbon steel grades such as EN 10216-2 P235GH, while chromium, nickel and copper are held as residuals of 0.30% maximum. Seamless tubes and pipe are made to EN 10216-2; plate for vessels and fabricated components is made to EN 10028-2.

16Mo3 is often treated as the European counterpart of ASTM A335 P1, but the two are not interchangeable: P1 carries 0.44–0.65% molybdenum, and the tensile and yield rules differ. EN 10216-2 also sets minimum yield strength by wall thickness, so heavier walls carry lower guaranteed yield values that must be used in design.

Tubes are delivered normalised (+N). EN 10216-2 allows two test categories: TC1 for standard testing and TC2 with additional non-destructive testing for more demanding service. Like other molybdenum steels without chromium, 16Mo3 is not intended for very long service at temperatures where graphitisation becomes a concern; higher temperatures call for chrome-moly grades such as 13CrMo4-5. Metals Fabrica confirms the EN 10216-2 test category, dimensions to EN 10220 and the inspection document type for 16Mo3 orders, with 3.2 available through a third-party inspector.

  • Standards: EN 10216-2 (seamless tube), EN 10028-2 (plate)
  • Material number: 1.5415
  • Delivery condition: normalised (+N)
  • Test categories: TC1 or TC2
TYPES & VARIANTS

Types of 16Mo3 Pipe

16Mo3 Seamless Tube to EN 10216-2

Hot-finished or cold-finished seamless tube ordered by outside diameter and wall, delivered normalised for boiler and superheater service.

16Mo3 Test Category TC1 and TC2

TC1 covers standard inspection; TC2 adds non-destructive testing of the tube body and is specified for more critical pressure parts.

16Mo3 Boiler Headers and Pipe

Larger-diameter seamless 16Mo3 pipe for headers and connecting pipework in steam generators designed to EN 12952 or similar codes.

16Mo3 Plate to EN 10028-2

Pressure-vessel plate in the same grade, used for drums, fabricated headers and welded components that complete a 16Mo3 system.

SPECIFICATIONS

16Mo3 Pipe Specifications

SpecificationDetails
Tube standardEN 10216-2 (seamless steel tubes for pressure purposes, elevated temperature)
Plate standardEN 10028-2
Material number1.5415
Former designation15Mo3 (DIN 17175)
Size range1/8" NB to 24" NB seamless
Wall thicknessSCH 10 to SCH 160, STD, XS, XXS, or metric OD × wall
Manufacturing typeSeamless, hot finished or cold finished
Delivery conditionNormalised (+N)
Test categoryTC1 or TC2 per EN 10216-2
Ends and lengthPlain or bevelled ends; random or cut lengths
DocumentationEN 10204 3.1 inspection certificate; EN 10204 3.2 on request

State the standard, test category, OD, wall and length in your enquiry.

CHEMICAL COMPOSITION

16Mo3 Pipe Chemical Composition

Weight %, cast analysis, maximum unless a range is shown.

16Mo3 to EN 10216-2 (tube)

GradeCSiMnPSCrMoNiCu
16Mo3 (1.5415)0.12 – 0.200.350.40 – 0.900.0250.0200.300.25 – 0.350.300.30

16Mo3 to EN 10028-2 (plate)

GradeCSiMnPSCrMoNiCu
16Mo3 (1.5415)0.12 – 0.200.350.40 – 0.900.0250.0100.300.25 – 0.350.300.30

EN 10028-2 also limits nitrogen and residual elements; confirm against the edition named in the order.

MECHANICAL PROPERTIES

16Mo3 Pipe Mechanical Properties

Room-temperature tensile requirements in MPa (N/mm²).

16Mo3 tube to EN 10216-2 (+N)

Wall thickness TUpper Yield Strength ReH, minTensile Strength RmElongation A, min (longitudinal / transverse)
T ≤ 16 mm280 MPa450 – 600 MPa22% / 20%
16 < T ≤ 40 mm270 MPa450 – 600 MPa22% / 20%
40 < T ≤ 60 mm260 MPa450 – 600 MPa22% / 20%

16Mo3 plate to EN 10028-2 (+N)

Thickness tUpper Yield Strength ReH, minTensile Strength RmElongation A, min
t ≤ 16 mm275 MPa440 – 590 MPa22%
16 < t ≤ 40 mm270 MPa440 – 590 MPa22%
40 < t ≤ 60 mm260 MPa440 – 590 MPa22%
EQUIVALENT GRADES

16Mo3 Equivalent Grades

GradeUNSEN / DINJISBSGB
16Mo3K11522 (A335 P1, approx.)16Mo3 (1.5415); DIN 15Mo3STPA 12–15MoG

Approximate equivalents only. ASTM A335 P1 and STPA 12 carry higher molybdenum than 16Mo3; equivalence must be approved by the designer.

APPLICATIONS

16Mo3 Pipe Applications

Boiler Superheaters and Headers

Superheater tubes, headers and connecting pipes in water-tube boilers built to European codes, where molybdenum adds strength at temperature.

Waste-to-Energy and Biomass Boilers

Pressure parts in moderate-temperature superheater and economiser sections of industrial boilers, where 16Mo3 is a common EN material choice.

Pressure Vessels and Heat Exchangers

Shells, nozzles and connecting pipework combining EN 10216-2 tube and EN 10028-2 plate in the same 1.5415 grade.

Refinery and Chemical Steam Systems

Steam and hot process lines in plants designed to EN 13480, where carbon steel strength at temperature is not sufficient.

WHY METALS FABRICA

Why Choose Metals Fabrica for 16Mo3 Pipe?

  • EN details confirmed: we check the EN 10216-2 grade, test category (TC1 or TC2), delivery condition and dimensions before quoting.
  • Yield by wall thickness: certificate values are reviewed against the EN 10216-2 limit for the actual wall thickness supplied.
  • Plate and tube together: 16Mo3 tube quoted with EN 10028-2 plate and alloy steel fittings where required.
  • Documentation support: EN 10204 3.1 certificates, and 3.2 with third-party inspection coordinated when requested.
FAQ

16Mo3 Pipe FAQs

16Mo3 (1.5415) is a molybdenum steel for pressure purposes at elevated temperature, with 0.12–0.20% carbon and 0.25–0.35% molybdenum. It is standardised for tubes in EN 10216-2 and for plate in EN 10028-2.

It is the closest ASTM grade but not a direct equivalent. P1 has 0.44–0.65% molybdenum and different tensile rules, so substitution needs engineering approval.

Under EN 10216-2 the minimum upper yield strength is 280 MPa for walls up to 16 mm, falling to 270 MPa and 260 MPa for thicker walls. Tensile strength is 450–600 MPa.

Test category TC2 includes additional non-destructive testing and inspection compared with TC1. The design code or purchaser specifies which category is needed.

Under the former German standard DIN 17175 the comparable grade was 15Mo3, with the same material number 1.5415.

REQUEST A QUOTE

Request a Quote for 16Mo3 Pipe

Send the EN standard, test category, OD, wall thickness, length, quantity and certificate type for 16Mo3 pipe or plate, and we will reply with price and availability.