Copper nickel pipe, also called cupronickel or CuNi pipe, is made from copper alloys containing 10% or 30% nickel with small, controlled additions of iron and manganese. In seawater these alloys form a thin, adherent protective film that keeps corrosion rates low, and the copper ions released from the surface discourage marine growth. That combination of corrosion and biofouling resistance makes copper nickel the traditional material for seawater piping on ships, offshore platforms and coastal plants.
Two grades cover most requirements. Copper nickel 90/10 (UNS C70600) is the economical general-purpose grade for seawater, firemain and cooling-water systems. Copper nickel 70/30 (UNS C71500) has higher strength and tolerates higher flow velocities, sand erosion and polluted water, and is chosen for condensers, desalination heat-recovery sections and more demanding service.
Seamless pipe is extruded and drawn, while larger diameters are welded from plate or strip. ASTM B466 covers seamless pipe and tube, ASTM B467 welded pipe and ASTM B111 condenser and heat-exchanger tube. Naval and offshore projects often specify EEMUA 144 (90/10 pipe in pressure series), BS 2871 or DIN 86019 instead, so the standard should be confirmed with the size. Metals Fabrica confirms whether your marine project follows ASTM, EEMUA 144, BS 2871 or DIN 86019 dimensions, as sizes are not interchangeable between these standards.
Extruded and drawn copper nickel pipe and tube without a weld seam, supplied annealed or light drawn for seawater and process lines.
Pipe welded from copper nickel strip or plate for larger diameters, commonly used for seawater intake, cooling and ballast mains.
Seamless 90/10 and 70/30 tubes in OD and wall (gauge) sizes for condensers, coolers, evaporators and feedwater heaters in marine and power service.
Copper nickel 90/10 pipe to the EEMUA 144 dimensional and composition series widely used in offshore and naval seawater systems.
CuNi10Fe1.6Mn tubes to DIN 86019 for shipbuilding and BS 2871 CN102 or CN107 tubes for marine and general engineering.
| Specification | Details |
|---|---|
| Pipe standards | ASTM B466 / ASME SB466 (seamless), ASTM B467 / ASME SB467 (welded) |
| Tube standards | ASTM B111 / ASME SB111 (seamless condenser and exchanger tube), ASTM B543 (welded exchanger tube) |
| Other standards | EEMUA 144 (90/10), BS 2871 Part 2 (CN102, CN107), DIN 86019 (CuNi10Fe1.6Mn) |
| UNS | C70600 (90/10), C71500 (70/30) |
| Size range | 1/4" NB to 24" NB |
| Wall thickness | SCH 10, 40, 80 and specified wall; EEMUA 144 pressure series |
| Manufacturing type | Seamless (extruded and drawn), welded |
| Temper / condition | Annealed (O61); light drawn on request |
| Ends | Plain end, bevelled end |
| Length | Single random, double random, cut length |
| Testing | Hydrostatic or eddy-current test per product standard; flattening and expansion tests where specified; PMI on request |
| Documentation | EN 10204 3.1 mill test certificate; EN 10204 3.2 with third-party inspection on request |
Copper nickel pipe sizes differ between ASTM, EEMUA and DIN standards. Confirm the standard, OD and wall in your enquiry.
| Grade | UNS | Cu | Ni | Fe | Mn | Pb | Zn |
|---|---|---|---|---|---|---|---|
| 90/10 | C70600 | Remainder | 9.0 – 11.0 | 1.0 – 1.8 | 1.0 | 0.05 | 1.0 |
| 70/30 | C71500 | Remainder | 29.0 – 33.0 | 0.40 – 1.0 | 1.0 | 0.05 | 1.0 |
Cu includes Ag and Ni includes Co. Tighter limits on Pb, Zn, C, P and S apply when the product is intended for subsequent welding; see each grade page.
| Grade | Tensile Strength, min | Yield Strength (0.5% Extension), min |
|---|---|---|
| 90/10 (C70600) | 260 MPa (38 ksi) | 90 MPa (13 ksi) |
| 70/30 (C71500) | 360 MPa (52 ksi) | 125 MPa (18 ksi) |
ASTM B111 tube and drawn tempers have different minimums. Confirm requirements against the standard and temper on your purchase order.
| Grade | UNS | Werkstoff Nr. | EN / DIN | JIS | BS |
|---|---|---|---|---|---|
| CuNi 90/10 | C70600 | 2.0872 | CuNi10Fe1Mn (CW352H) | C7060 | CN102 |
| CuNi 70/30 | C71500 | 2.0882 | CuNi30Mn1Fe (CW354H) | C7150 | CN107 |
Equivalents are approximate; EEMUA 144 and DIN 86019 90/10 have tighter iron and manganese ranges than ASTM C70600. Order to the standard named in your specification.
Seawater cooling, firemain, ballast and sanitary systems, where 90/10 resists seawater corrosion and marine fouling over long service lives.
Firewater ring mains, deluge and seawater lift piping where low corrosion rates and resistance to marine growth reduce maintenance.
Brine heater, heat-recovery and evaporator tubing in multi-stage flash plants, with 70/30 used in the hotter and more erosive sections.
Condenser and cooling-water tubes for coastal power plants that use seawater or brackish water, where copper nickel resists both corrosion and fouling.
Small-bore 90/10 tube for hydraulic, brake and fuel lines where formability and resistance to road salt are needed.
90/10 contains about 10% nickel and is the standard grade for seawater piping. 70/30 contains about 30% nickel, giving higher strength and better resistance to high flow velocity, erosion and polluted seawater, at a higher cost.
ASTM B466 covers seamless pipe and tube, ASTM B467 welded pipe and ASTM B111 condenser and heat-exchanger tube. EEMUA 144, BS 2871 and DIN 86019 are also widely used in marine and offshore projects.
Copper nickel forms a protective surface film in seawater that keeps corrosion rates very low, and it naturally resists attachment of marine organisms. It also has good thermal conductivity for heat exchangers.
Yes. Design guidance usually limits seawater velocity to about 3.5 m/s for 90/10 in larger pipe and somewhat higher for 70/30, but the limit depends on pipe diameter and the design code used.
State the grade, product standard, seamless or welded, OD and wall or NB and schedule, temper, length, end finish, quantity, tests and certificates, and the delivery location.