Inconel 718 bar is the most widely used precipitation-hardened nickel alloy bar. Niobium, titanium and aluminium in the nickel-chromium-iron matrix form fine strengthening precipitates during ageing, giving a minimum yield strength of 1034 MPa with good toughness from cryogenic temperatures to about 650 °C. Bar in 718 is the standard stock for high-strength bolts, shafts, discs and oilfield components.
The heat-treatment condition is the key ordering decision. AMS 5662 bar is delivered solution heat treated, around 968 °C, so it is soft enough to rough machine; the part is then aged, typically 718 °C for 8 hours, furnace cooled to 621 °C and held for a total of 18 hours, and must then meet the aged properties. AMS 5663 bar is delivered already solution treated and aged, ready for finish machining to a final hardness of 331 HB minimum. ASTM B637 covers 718 bar and forgings for industrial high-temperature service with similar aged requirements, and API 6A718 is often specified for oilfield equipment.
Aged 718 is hard and abrasive to machine, so many buyers rough machine in the solution-treated condition and finish after ageing. Metals Fabrica supplies 718 bar with the specification, revision and condition confirmed at enquiry stage. The same alloy is offered as Inconel 718 sheet and plate and Inconel 718 tubing.
Soft bar delivered solution heat treated for rough machining or forging, then aged by the user to reach full strength in the finished part.
Bar delivered fully aged with certified tensile, hardness and stress-rupture results, ready for finish machining of bolts, shafts and rings.
Industrial bar and forging stock for high-temperature service in power, petrochemical and turbine equipment, ordered solution treated or aged.
Bar processed to the oilfield specification with controlled hardness and microstructure for wellhead, valve and downhole components in sour service.
Precision-ground bar held to close tolerance for aerospace fasteners and thread-rolled studs, reducing machining of a hard, abrasive alloy.
| Specification | Details |
|---|---|
| Product specifications | ASTM B637 / ASME SB637; AMS 5662; AMS 5663; API 6A718 on request |
| UNS / Werkstoff Nr. | N07718 / 2.4668 |
| Shapes | Round, hex, square, flat, forged blocks |
| Size range | 3 mm to 500 mm round; hex and square to order |
| Length | 1 to 6 m random, fixed and cut lengths |
| Condition | Solution treated (AMS 5662); solution treated and precipitation hardened (AMS 5663, B637) |
| Ageing treatment | 718 °C (1325 °F) 8 h, furnace cool to 621 °C (1150 °F), hold to 18 h total, air cool |
| Finish | Black, peeled, turned, centreless ground |
| Tolerance | h9 or h11 typical for ground bar; k12 for peeled bar |
| Testing | Tensile, hardness, grain size and stress-rupture per specification; ultrasonic testing and PMI |
| Documentation | EN 10204 3.1 certificate listing specification revision and melting route; EN 10204 3.2 on request |
Name the specification and revision on your order. AMS 5662 bar is certified on aged test samples even though it is shipped solution treated.
| Grade | UNS | Ni | Cr | Fe | Nb+Ta | Mo | Ti | Al | Co | C | Mn | Si | Cu | B |
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| 718 | N07718 | 50.0 – 55.0 | 17.0 – 21.0 | Remainder | 4.75 – 5.50 | 2.80 – 3.30 | 0.65 – 1.15 | 0.20 – 0.80 | 1.00 | 0.08 | 0.35 | 0.35 | 0.30 | 0.006 |
P and S are limited to 0.015 each. AMS specifications add limits on trace elements; check the revision ordered.
| Specification / Condition | Tensile Strength, min | Yield Strength (0.2% Offset), min | Elongation in 4D, min | Reduction of Area, min | Hardness |
|---|---|---|---|---|---|
| AMS 5662, solution treated (as supplied) | – | – | – | – | 277 HB max |
| AMS 5662 after ageing / AMS 5663, solution treated and aged | 1276 MPa (185 ksi) | 1034 MPa (150 ksi) | 12% | 15% | 331 HB min |
| ASTM B637, solution treated and aged | 1275 MPa (185 ksi) | 1034 MPa (150 ksi) | 12% | 15% | 331 HB min |
Aged bar is also tested for stress rupture at 649 °C (1200 °F). Typical density 8.19 g/cm³; melting range 1260–1336 °C.
| Grade | UNS | Werkstoff Nr. | EN | JIS | BS | AFNOR | GOST |
|---|---|---|---|---|---|---|---|
| Inconel 718 | N07718 | 2.4668 | NiCr19Fe19Nb5Mo3 | NCF 718 | – | NC19FeNb | – |
Equivalents are approximate. Aerospace and oilfield orders must follow the named AMS, API or customer specification.
AMS 5662 and 5663 bar and forging stock for compressor and turbine shafts, discs and spacers operating at high stress up to about 650 °C.
Studs, bolts and nuts for turbine casings, hot flanges and pressure equipment, where aged 718 resists relaxation and keeps preload at temperature.
Hangers, valve stems, packer mandrels and drilling tools in high-pressure sour wells, where strength and resistance to hydrogen sulphide are both required.
Turbopump shafts, fittings and fasteners that must keep strength and toughness at liquid hydrogen and liquid oxygen temperatures.
Extrusion dies, hot shear blades and forming tools that need high hot strength and resistance to softening during repeated heating.
AMS 5662 covers 718 bar, forgings and rings delivered solution heat treated, which the user ages after machining. AMS 5663 covers the same products delivered solution treated and aged, ready for finish machining. Both require the aged material to meet the same minimum properties.
The standard ageing cycle is 718 °C for 8 hours, furnace cooling to 621 °C, and holding at 621 °C until the total ageing time reaches 18 hours, followed by air cooling. The specification ordered may set different solution or ageing temperatures.
Aged 718 bar to AMS 5663 or ASTM B637 must reach a minimum of 331 HB, roughly 36 HRC. Oilfield specifications such as API 6A718 also set a maximum hardness for sour service.
Many shops rough machine in the solution-treated condition, age the part, then finish machine to remove distortion and achieve final tolerances. Machining fully aged bar is possible but slower and harder on tooling.
Yes, when processed and hardness-controlled to the limits of NACE MR0175 / ISO 15156 or API 6A718. Standard aerospace-aged bar may exceed sour-service hardness limits, so the oilfield requirement must be stated.