Carbon steel bar is iron with up to roughly 0.5% carbon and small, controlled amounts of manganese and silicon, without the deliberate chromium or molybdenum additions of alloy steel. Carbon and manganese set the strength; the heat treatment and the standard set the toughness and hardness. It is the most economical bar material for pressure parts, shafts, studs and fabricated components in non-corrosive or coated service.
For piping components, buyers usually order bar certified to a forging standard. ASTM A105 bar is used to machine small flanges, fittings and valve parts for ambient and elevated-temperature service. ASTM A350 LF2 bar has similar strength but is heat treated and Charpy impact tested at −46 °C (Class 1) or −18 °C (Class 2) for low-temperature lines. For general engineering, structural bar to ASTM A36 or IS 2062 and medium-carbon EN 10083 C45 for shafts and gears are more common.
A105 and A350 allow small hollow cylindrical parts to be machined from hot-rolled or forged bar when the part axis runs parallel to the bar’s flow lines, so bar stock certified to these standards is widely used for machined components. Metals Fabrica supplies carbon steel bar to the standard on your order and checks that the heat treatment and tests match it. Matching carbon steel flanges and carbon steel pipe fittings are also available.
Hot-rolled or forged carbon steel bar certified to A105 for machining small flanges, couplings, plugs and valve parts used in ambient and high-temperature piping.
Normalised or quenched and tempered bar with Charpy impact testing, used for flanges and fittings in cold-climate, LPG and refrigerated service.
Medium-carbon EN 10083 bar supplied normalised or quenched and tempered, peeled or ground, for shafts, pins, spindles and gears.
A36 and IS 2062 hot-rolled bars for base plates, supports, anchor rods and general fabrication where weldability matters more than hardness.
Hexagon and square sections for nuts, unions, bushes and machined blocks, cut to length or supplied in random lengths.
Large forged carbon steel sections for valve bodies, tube sheets and heavy flanges, normalised and ultrasonically tested when the order requires it.
| Specification | Details |
|---|---|
| Forging standards (bar stock) | ASTM A105 / ASME SA105; ASTM A350 / ASME SA350 LF2 Class 1 and Class 2 |
| Engineering and structural standards | EN 10083-2 C45; ASTM A36; IS 2062 |
| Shapes | Round, hexagon, square, flat, rectangular; forged blocks |
| Size range | 3 mm to 500 mm round; hex and square to order |
| Length | 1 to 6 m random, fixed and cut lengths |
| Condition | As rolled, normalised, normalised and tempered, quenched and tempered (as the standard permits) |
| Finish | Black, bright drawn, peeled, turned, centreless ground |
| Tolerance | h9, h11 or k12 (typical for bright bar) |
| Testing | Tensile, hardness, Charpy impact (A350), ultrasonic testing and PMI on request |
| Documentation | EN 10204 3.1 mill test certificate; EN 10204 3.2 on request |
Confirm the standard, class, size, heat treatment and tests in your enquiry.
| Grade | UNS | C | Mn | Si | P | S | Cr | Ni | Mo | Other |
|---|---|---|---|---|---|---|---|---|---|---|
| ASTM A105 | K03504 | 0.35 | 0.60 – 1.05 | 0.10 – 0.35 | 0.035 | 0.040 | 0.30 | 0.40 | 0.12 | Cu 0.40; V 0.08 |
| ASTM A350 LF2 | K03011 | 0.30 | 0.60 – 1.35 | 0.15 – 0.30 | 0.035 | 0.040 | 0.30 | 0.40 | 0.12 | Cu 0.40; V 0.08; Nb 0.02 |
| ASTM A36 (bars) | K02600 | 0.26 – 0.29 (by size) | 0.60 – 0.90 (over 19 mm) | 0.40 | 0.04 | 0.05 | – | – | – | Cu 0.20 min when copper steel is specified |
| EN 10083-2 C45 | – | 0.42 – 0.50 | 0.50 – 0.80 | 0.40 | 0.030 | 0.035 | 0.40 | 0.40 | 0.10 | Cr + Mo + Ni 0.63 |
A105 and LF2 also limit Cu + Ni + Cr + Mo + V to 1.00% and Cr + Mo to 0.32%. A36 carbon maximum rises with bar size.
| Grade | Tensile Strength | Yield Strength, min | Elongation in 50 mm, min | Hardness / Impact |
|---|---|---|---|---|
| ASTM A105 | 485 MPa (70 ksi) min | 250 MPa (36 ksi) | 22% (round specimen) | 187 HBW max |
| ASTM A350 LF2 Class 1 | 485 – 655 MPa (70 – 95 ksi) | 250 MPa (36 ksi) | 22% (round specimen) | Charpy 20 J avg at −46 °C |
| ASTM A350 LF2 Class 2 | 485 – 655 MPa (70 – 95 ksi) | 250 MPa (36 ksi) | 22% (round specimen) | Charpy 20 J avg at −18 °C |
| ASTM A36 (bars) | 400 – 550 MPa (58 – 80 ksi) | 250 MPa (36 ksi) | 23% | – |
| EN 10083-2 C45 +N (16 < d ≤ 100 mm) | 580 MPa min | 305 MPa | 16% | – |
Density of carbon steel is typically 7.85 g/cm³ (typical, not a requirement). C45 properties depend on section size and condition; quenched and tempered values are higher.
| Grade | UNS | EN / DIN | JIS | BS | GB | IS |
|---|---|---|---|---|---|---|
| ASTM A105 | K03504 | P250GH (1.0460) | SFVC 2A | – | – | – |
| ASTM A350 LF2 | K03011 | P285QH (1.0478) | SFL 2 | – | – | – |
| ASTM A36 | K02600 | S275JR (1.0044) | SS400 | – | Q235B | IS 2062 E250 |
| C45 | G10450 (AISI 1045) | C45 (1.0503) | S45C | 080M46 | 45 | 45C8 |
Equivalents are approximate and differ in chemistry limits, testing and impact requirements. Order to the standard named in your specification.
A105 and LF2 bar for machining socket-weld and threaded fittings, small flanges, bonnets and valve stems in refinery, power and utility piping.
Impact-tested LF2 bar for components in LPG, ammonia and cold-climate plants where carbon steel must stay tough below zero.
Normalised or hardened C45 bar for drive shafts, axles, pins and gear blanks that need higher strength than mild steel.
A36 and IS 2062 round and flat bars for frames, supports, anchor bolts and platforms in plants and buildings.
Bright carbon steel bar for hydraulic cylinder ends, couplings, bushes and turned parts in machinery, where close tolerance reduces machining time.
ASTM A105 permits hollow cylindrical parts of limited size to be machined from hot-rolled or forged bar when the part axis is approximately parallel to the bar’s flow lines. Elbows, tees and similar shapes may not be machined directly from bar stock.
Both are carbon-manganese steels with a 250 MPa minimum yield. LF2 must be heat treated and Charpy impact tested at low temperature, while A105 has no impact requirement and is intended for ambient and elevated-temperature service.
Medium-carbon grades such as EN 10083 C45 (similar to AISI 1045) are common for shafts and pins because they can be normalised or quenched and tempered to higher strength. A105 and A36 are lower in carbon and mainly used for pressure parts and fabrication.
A105N is a trade term for A105 material supplied in the normalised condition. It is not a separate ASTM grade, so the normalising requirement should be written into the purchase order.
Bar is normally supplied with an EN 10204 3.1 mill test certificate showing heat number, chemistry, heat treatment and test results. An EN 10204 3.2 certificate with third-party witness can be arranged when specified.