SS 317 flanges are forged from an austenitic stainless steel with 18.0–20.0% chromium, 11.0–15.0% nickel and 3.0–4.0% molybdenum, designated F317 (UNS S31700) in ASTM A182. The extra molybdenum, roughly a third more than in 316, raises the pitting resistance equivalent number and improves resistance to sulphuric, acetic and phosphoric acids and to halide-bearing process streams.
F317L (UNS S31703) restricts carbon to 0.030%, which protects welds from sensitisation and is why it is the variant most often specified. Because the higher molybdenum content tends to segregate in weld metal, fabricators often use an over-alloyed filler so that the weld is as corrosion resistant as the flange. Minimum strengths follow the 316 pattern: 515 MPa tensile and 205 MPa yield for F317, and 485 MPa and 170 MPa for F317L.
Specify 317L when SS 316L flanges show pitting or are close to their limit, but before moving to 6Mo stainless or nickel alloys. Metals Fabrica supplies F317 and F317L flanges in weld neck, slip-on, blind and other types, with matching SS 317 / 317L pipe and SS 317 / 317L pipe fittings.
The usual 317L flange for acid and scrubber piping, with the hub butt-welded to the pipe and the bore matched to SCH 10S or 40S wall thickness.
For low-pressure chemical and effluent lines where fillet welds are acceptable; the low-carbon grade keeps both welds free of chromium carbide precipitation.
Blanks for vessel nozzles and line ends in molybdenum-sensitive service, where a 316 blind could become the weak point against pitting under the gasket.
317L stub ends carry the corrosive contact while the loose backing flange, which is not wetted, carries the bolt load and can rotate for alignment.
Forgings that meet the 0.030% carbon limit of F317L and the 515 MPa tensile minimum of F317, for piping classes that list either grade.
| Specification | Details |
|---|---|
| Material standard | ASTM A182 / ASME SA182 F317, F317L |
| UNS | S31700 (F317), S31703 (F317L) |
| Dimension standards | ASME B16.5, ASME B16.47 Series A / B, ASME B16.48, EN 1092-1 |
| Size range | 1/2" to 24" NB (ASME B16.5); 26" to 48" NB and larger (ASME B16.47) |
| Pressure class | Class 150, 300, 600, 900, 1500, 2500; PN 6 to PN 100 |
| Flange types | Weld neck, slip-on, blind, socket weld, threaded, lap joint, orifice, reducing |
| Facing | Raised face (RF), flat face (FF), ring type joint (RTJ) |
| Face finish | Serrated 125–250 µin AARH; smooth finish on request |
| Heat treatment | Solution annealed at 1040 °C (1900 °F) minimum, rapidly cooled |
| Testing | Chemical analysis, tensile, PMI, dimensional; IGC to ASTM A262 and pitting test to ASTM G48 on request |
| Documentation | EN 10204 3.1 certificate; EN 10204 3.2 on request |
Confirm grade, flange type, size, class, facing and bore schedule in your enquiry.
| Grade | UNS | C | Mn | Si | P | S | Cr | Ni | Mo | N |
|---|---|---|---|---|---|---|---|---|---|---|
| F317 | S31700 | 0.08 | 2.00 | 1.00 | 0.045 | 0.030 | 18.0 – 20.0 | 11.0 – 15.0 | 3.0 – 4.0 | 0.10 |
| F317L | S31703 | 0.030 | 2.00 | 1.00 | 0.045 | 0.030 | 18.0 – 20.0 | 11.0 – 15.0 | 3.0 – 4.0 | 0.10 |
| Grade | Density | Melting Range | Tensile Strength, min | Yield Strength (0.2% Offset), min | Elongation in 50 mm, min | Reduction of Area, min |
|---|---|---|---|---|---|---|
| F317 | 8.00 g/cm³ | 1370 – 1400 °C | 515 MPa (75 ksi) | 205 MPa (30 ksi) | 30% | 50% |
| F317L | 8.00 g/cm³ | 1370 – 1400 °C | 485 MPa (70 ksi) | 170 MPa (25 ksi) | 30% | 50% |
Density and melting range are typical values, not specification requirements.
| Grade | UNS | Werkstoff Nr. | EN | JIS | BS | AFNOR | GOST |
|---|---|---|---|---|---|---|---|
| SS 317 | S31700 | 1.4449 | X3CrNiMo18-12-3 | SUS 317 | 317S16 | – | – |
| SS 317L | S31703 | 1.4438 | X2CrNiMo18-15-4 | SUS 317L | 317S12 | Z3CND19-15-04 | – |
Equivalents are approximate; EN 1.4438 has a higher nickel range than ASTM 317L. Order to the standard named in your specification.
Absorber, slurry and reagent lines in FGD scrubbers, where acidic, chloride-bearing slurry pits 316L but does not yet justify nickel alloys.
Bleach-filtrate and chemical lines where the extra molybdenum of 317L improves resistance to pitting and crevice corrosion in chloride-containing liquors.
Process and transfer lines in acid production and recovery, where F317L lasts longer than 316L in hot or contaminated acid.
Batch reactor and transfer piping exposed to changing acids and halides, where 317L gives margin against unpredictable process conditions.
Process-side connections on exchangers handling corrosive condensates with chlorides, where pitting under gaskets is the main failure risk.
317L contains 3.0–4.0% molybdenum and 18.0–20.0% chromium, against 2.00–3.00% and 16.0–18.0% in 316L. The higher alloy content gives better resistance to pitting, crevice corrosion and several acids, at a higher price.
Using PREN = Cr + 3.3Mo + 16N, typical 317L compositions give a value of about 28 to 30, compared with about 24 for typical 316L. The minimum composition gives a lower figure, so check actual certificate values when PREN is specified.
ER317L is the matching filler. For the best corrosion resistance, many procedures use a more highly alloyed filler such as ERNiCrMo-3 to offset molybdenum segregation in the weld metal.
Most 317 flanges are welded into corrosive service, where low carbon protects the heat-affected zone from sensitisation. F317 is used mainly where its higher minimum strength is needed and welding conditions allow.
Besides the A182 chemical and tensile tests, buyers commonly add PMI, intergranular corrosion testing to ASTM A262 and pitting tests to ASTM G48. Test methods and acceptance criteria should be stated on the order.