Carbon steel flanges are the most widely used pipe flanges in refineries, utilities, water systems and pipelines. They are forged from killed carbon-manganese steel, heat treated where the material standard requires it, and machined to the bore, facing and bolt pattern of ASME B16.5, B16.47, MSS SP-44 or EN 1092-1. Choosing a grade is mainly a question of service temperature, toughness and required strength rather than corrosion resistance.
ASTM A105 is the default for ambient and elevated-temperature piping, with 485 MPa minimum tensile and 250 MPa yield. ASTM A350 LF2 has similar strength but is always heat treated and Charpy tested, at −46 °C for Class 1, for low-temperature service. ASTM A694 grades F42 to F70 give minimum yields from 290 to 485 MPa to match high-strength line pipe, and ASTM A181 Class 60 and 70 cover general-purpose forgings.
The flange grade should follow the pipe grade and design temperature: A105 with A106 Grade B pipe, LF2 with A333 Grade 6, and A694 with API 5L X-grades. Metals Fabrica supplies carbon steel flanges across these standards, reviews type, class, facing and bore against your specification, and can quote matching carbon steel pipe and fittings in the same enquiry.
Tapered-hub flanges butt-welded to the pipe and bored to its schedule. Specified for high-pressure, high-temperature and fatigue-loaded lines where the weld must be radiographed.
Lower-cost flanges that slip over the pipe and are fillet-welded on both sides. Common on water, air and utility headers in Class 150 and 300.
Solid flanges that close line ends, valve outlets and vessel nozzles, and allow later extension of the line or access for internal inspection.
Small-bore flanges for instrument, drain and utility connections. Threaded versions with NPT threads suit non-hazardous lines where welding on site is not wanted.
Large-diameter weld neck and blind flanges, usually in A694 grades, with the weld end bored and bevelled to match the wall thickness of high-yield line pipe.
A105 or LF2 orifice flange sets to ASME B16.36 for flow metering, and spectacle blinds, spades and spacers to ASME B16.48 for line isolation.
| Specification | Details |
|---|---|
| Material standards | ASTM A105 / ASME SA105; ASTM A350 / ASME SA350 LF2 Class 1 / 2; ASTM A694 F42 – F70; ASTM A181 Class 60 / 70 |
| Dimension standards | ASME B16.5, ASME B16.47 Series A / B, ASME B16.36, ASME B16.48, MSS SP-44, EN 1092-1 |
| Size range | 1/2" to 24" NB (ASME B16.5); 26" to 48" NB and larger (ASME B16.47, MSS SP-44) |
| Pressure class | Class 150, 300, 400, 600, 900, 1500, 2500; PN 6 to PN 100 (EN 1092-1) |
| Flange types | Weld neck, slip-on, blind, socket weld, threaded, lap joint, long weld neck, orifice, spectacle blind, reducing |
| Facing | Raised face (RF), flat face (FF), ring type joint (RTJ), tongue and groove, male and female |
| Face finish | Serrated 125–250 µin AARH (3.2–6.3 µm Ra); smooth finish on request |
| Heat treatment | A105: as forged or heat treated (mandatory above Class 300); LF2 and A694: normalised, normalised and tempered, or quenched and tempered |
| Surface protection | Rust-preventive oil or varnish; painting or hot-dip galvanising on request |
| Testing | Chemical analysis, tensile, hardness, Charpy impact (LF2, and A694 where specified), UT and MPI on request |
| Documentation | EN 10204 3.1 certificate; EN 10204 3.2 with third-party inspection on request |
State the material standard, class or grade, impact temperature where relevant, and the dimensional standard in your enquiry.
| Grade | C | Mn | P | S | Si | Cu | Ni | Cr | Mo | V |
|---|---|---|---|---|---|---|---|---|---|---|
| A105 | 0.35 | 0.60 – 1.05 | 0.035 | 0.040 | 0.10 – 0.35 | 0.40 | 0.40 | 0.30 | 0.12 | 0.08 |
| A350 LF2 | 0.30 | 0.60 – 1.35 | 0.035 | 0.040 | 0.15 – 0.30 | 0.40 | 0.40 | 0.30 | 0.12 | 0.08 |
| A694 F42 – F70 | 0.26 | 1.60 | 0.025 | 0.025 | 0.15 – 0.35 | – | – | – | – | – |
| A181 Class 60 / 70 | 0.35 | 1.10 | 0.05 | 0.05 | 0.10 – 0.35 | – | – | – | – | – |
A350 LF2 also limits Nb to 0.02%. Residual-element totals and manganese-for-carbon allowances are given on each grade page.
| Grade | Tensile Strength, min | Yield Strength, min | Elongation in 50 mm, min | Hardness / Impact |
|---|---|---|---|---|
| A105 | 485 MPa (70 ksi) | 250 MPa (36 ksi) | 22% (round specimen); 30% (strip) | 137 – 187 HBW |
| A350 LF2 Class 1 | 485 – 655 MPa (70 – 95 ksi) | 250 MPa (36 ksi) | 22% | Charpy V-notch at −46 °C (−50 °F) |
| A350 LF2 Class 2 | 485 – 655 MPa (70 – 95 ksi) | 250 MPa (36 ksi) | 22% | Charpy V-notch at −18 °C (0 °F) |
| A694 F42 – F70 | 415 – 565 MPa (60 – 82 ksi) | 290 – 485 MPa (42 – 70 ksi) | 20% (F70: 18%) | Impact by agreement |
| A181 Class 60 | 415 MPa (60 ksi) | 205 MPa (30 ksi) | 22% | – |
| A181 Class 70 | 485 MPa (70 ksi) | 250 MPa (36 ksi) | 18% | – |
Density of carbon steel is typically 7.85 g/cm³. See each grade page for reduction of area, impact energies and the full A694 grade table.
| Grade | UNS | EN (approx.) | JIS (approx.) | Matching pipe grade |
|---|---|---|---|---|
| A105 | K03504 | P250GH (1.0460) | SFVC 2A | ASTM A106 Gr B |
| A350 LF2 | K03011 | P285QH (1.0478) | SFL 2 | ASTM A333 Gr 6 |
| A694 F52 | – | – | – | API 5L X52 / L360 |
| A694 F65 | – | – | – | API 5L X65 / L450 |
| A181 Class 70 | – | – | SF490A | ASTM A53 Gr B / A106 Gr B |
Equivalents are approximate and differ in heat treatment, impact and residual-element requirements. Order to the standard named in your specification.
A105 weld neck and blind flanges on hydrocarbon process, steam and utility lines operating from ambient temperature up to the B16.5 limits for carbon steel.
A694 flanges at pig launchers, receivers, valve stations and tie-ins, matched to the yield strength of the API 5L line pipe they are welded to.
A350 LF2 Class 1 flanges on refrigerated storage, loading and process lines where design metal temperatures fall below the range of A105.
Feedwater, cooling water, fuel-oil and auxiliary steam connections in thermal and combined-cycle plants, typically in A105 to ASME B16.5.
Slip-on and blind flanges on water mains, pumping stations and fire-water ring mains, often with flat faces to mate with cast iron valves.
Nozzle flanges on vessels, heat exchangers, compressor and pump skids, where the forging grade must match the vessel design code.
Both have 485 MPa minimum tensile and 250 MPa minimum yield. LF2 must be heat treated and Charpy impact tested, at −46 °C for Class 1 or −18 °C for Class 2, which makes it suitable for low-temperature service; A105 has no impact requirement.
High-pressure transmission pipelines in API 5L X-grade pipe normally use ASTM A694 flanges. The A694 grade is chosen so its minimum yield matches the pipe, for example F52 with X52 or F65 with X65.
ASME B16.5 rates A105 into the high-temperature range but warns that prolonged exposure above about 425 °C can cause graphitisation. At the low end, A105 is usually limited to about −29 °C unless impact testing is added, which is why LF2 is used for colder service.
A350 LF2 and A694 flanges are always heat treated. A105 may be supplied as forged, but heat treatment is mandatory for flanges above Class 300 and certain special designs; many buyers specify normalised A105 for all classes.
Give the material standard and grade or class, flange type, size, pressure class or PN, facing, bore schedule, dimensional standard, coating, quantity, tests and certificates required, and the delivery location.