Titanium flanges combine low weight with near-immunity to corrosion in seawater, brines, wet chlorine and many oxidising chemicals. A tightly adherent titanium oxide film protects the metal even at high flow velocities, so titanium flanges are used where copper alloys, stainless steels and even some nickel alloys would pit, crack or erode. Titanium’s density is about 57% of steel’s, which matters on offshore topsides and in rotating or suspended equipment.
ASTM B381 covers titanium forgings, with grades prefixed F. F2 (UNS R50400) is commercially pure titanium and the default for corrosion service. F5 (Ti-6Al-4V, UNS R56400) is an alpha-beta alloy with roughly two and a half times the tensile strength of F2, used where strength matters more than formability. F7 adds 0.12–0.25% palladium to F2 for better resistance to reducing acids and crevice corrosion in hot brines, and F12 adds small amounts of molybdenum and nickel as a lower-cost alternative with higher strength than F2.
Titanium flanges are machined from annealed B381 forgings; lap joint designs with titanium stub ends and steel backing flanges are common to save cost. Metals Fabrica supplies titanium flanges with matching titanium pipe and titanium pipe fittings, confirming grade and design before quoting.
Commercially pure titanium flanges butt-welded to Grade 2 pipe for seawater, chlorine and chemical lines needing a full-penetration joint.
Titanium stub end in contact with the process fluid and a carbon or stainless backing flange, the most economical titanium flanged joint.
High-strength Ti-6Al-4V flanges for offshore, subsea and high-pressure equipment where weight saving and mechanical strength are both design requirements.
Solid Grade 2 or Grade 5 titanium blanks for closing seawater headers, heat exchanger channels and vessel nozzles without a dissimilar metal in contact with the fluid.
Fillet-welded flanges for low-pressure seawater and chemical lines; welding requires full inert gas shielding of both faces to prevent oxygen and nitrogen contamination.
| Specification | Details |
|---|---|
| Material standard | ASTM B381 / ASME SB381 (titanium and titanium alloy forgings) |
| Grades and UNS | F2 (R50400), F5 (R56400), F7 (R52400), F12 (R53400) |
| Dimension standards | ASME B16.5, ASME B16.47 Series A / B, ASME B16.36, ASME B16.48, EN 1092-1 |
| Size range | 1/2" NB to 48" NB and larger |
| Pressure class | Class 150 to 2500; PN 6 to PN 100 |
| Flange types | Weld neck, slip-on, blind, lap joint with stub end, socket weld, threaded, orifice, spectacle blind |
| Facing | RF, FF, RTJ |
| Condition | Annealed |
| Testing | Chemical analysis including O, N, H; tensile, ultrasonic, dye penetrant and dimensional inspection |
| Documentation | EN 10204 3.1 mill test certificate; EN 10204 3.2 with third-party inspection on request |
State grade, type, pressure class, facing and bore in your enquiry.
| Grade | UNS | N | C | H | Fe | O | Al | V | Other | Ti |
|---|---|---|---|---|---|---|---|---|---|---|
| F2 | R50400 | 0.03 | 0.08 | 0.015 | 0.30 | 0.25 | – | – | – | Balance |
| F5 | R56400 | 0.05 | 0.08 | 0.015 | 0.40 | 0.20 | 5.5 – 6.75 | 3.5 – 4.5 | – | Balance |
| F7 | R52400 | 0.03 | 0.08 | 0.015 | 0.30 | 0.25 | – | – | Pd 0.12 – 0.25 | Balance |
| F12 | R53400 | 0.03 | 0.08 | 0.015 | 0.30 | 0.25 | – | – | Mo 0.2 – 0.4; Ni 0.6 – 0.9 | Balance |
| Grade | Tensile Strength, min | Yield Strength (0.2% Offset) | Elongation in 4D, min | Reduction of Area, min | Density |
|---|---|---|---|---|---|
| F2 | 345 MPa (50 ksi) | 275 – 450 MPa (40 – 65 ksi) | 20% | 30% | 4.51 g/cm³ |
| F5 | 895 MPa (130 ksi) | 828 MPa (120 ksi) min | 10% | 25% | 4.43 g/cm³ |
| F7 | 345 MPa (50 ksi) | 275 – 450 MPa (40 – 65 ksi) | 20% | 30% | 4.51 g/cm³ |
| F12 | 483 MPa (70 ksi) | 345 MPa (50 ksi) min | 18% | 25% | 4.51 g/cm³ |
Density is a typical value, not a specification requirement.
| Grade | UNS | Werkstoff Nr. | EN / DIN | JIS | BS |
|---|---|---|---|---|---|
| Titanium Grade 2 (F2) | R50400 | 3.7035 | Ti 2 | Class 2 | – |
| Titanium Grade 5 (F5) | R56400 | 3.7165 | TiAl6V4 | Class 60 | – |
| Titanium Grade 7 (F7) | R52400 | 3.7235 | Ti 2 Pd | Class 12 | – |
| Titanium Grade 12 (F12) | R53400 | – | – | – | – |
Equivalents are approximate; oxygen and iron limits vary between standards. Order to the standard named in your specification.
Firewater, seawater lift and cooling flanges on platforms and FPSOs, where titanium resists seawater at high velocity and saves topside weight.
Wet chlorine, chlorine dioxide and hypochlorite lines, where Grade 2 titanium has very low corrosion rates compared with most metals.
Brine heater and seawater connections in thermal and membrane plants; Grade 7 or Grade 12 for hot brines prone to crevice corrosion.
Channel and nozzle flanges for titanium-tubed seawater condensers and plate heat exchangers, avoiding a galvanic mismatch between the flanges and the tubes.
Process lines for nitric acid, oxidising chlorides and hydrometallurgical leach solutions, with Pd-bearing Grade 7 for reducing conditions.
ASTM B381 / ASME SB381 covers titanium and titanium alloy forgings, including flanges, with grades designated F2, F5, F7, F12 and others. Dimensions follow ASME B16.5, B16.47 or EN 1092-1.
Grade 2 is commercially pure titanium with 345 MPa minimum tensile strength and the best corrosion resistance and weldability. Grade 5 (Ti-6Al-4V) reaches 895 MPa minimum tensile and is chosen where strength is critical.
In hot chloride brines and mildly reducing acids, Grade 2 can suffer crevice corrosion. Palladium-bearing Grade 7 and molybdenum-nickel Grade 12 resist this better, with Grade 12 also offering higher strength.
Only the titanium stub end touches the fluid, so the loose backing flange can be carbon or stainless steel. This reduces cost and simplifies bolt-hole alignment, provided the backing flange is protected against external corrosion.