Inconel pipe fittings are elbows, tees, reducers, caps and stub ends made from nickel-chromium alloys such as Inconel 600 and 625, together with the nickel-iron-chromium Incoloy alloys 800, 800H, 800HT and 825. They complete Inconel and Incoloy pipe systems that must resist oxidation, carburisation, chloride stress corrosion cracking or aggressive acids where stainless steel would fail.
Butt-weld fittings are covered by ASTM B366 / ASME SB366, which gives each alloy its own grade: WPNCI for alloy 600, WPNCMC for 625, WPNIC, WPNIC10 and WPNIC11 for 800, 800H and 800HT, and WPNICMC for 825. B366 does not set its own chemistry or tensile limits; the fitting must meet the requirements of the pipe, plate or bar specification it is made from. Class letters show construction and examination: WP-S is seamless, WP-W welded with radiography of fabrication welds, WP-WX fully radiographed and WP-WU ultrasonically examined, while CR classes follow the lighter MSS SP-43 dimensions. Forged socket-weld and threaded fittings are made from ASTM B564 forgings.
Alloy choice depends on the service: 625 for seawater, acids and high strength, 825 for sulphuric and phosphoric acid and sour service, 600 for caustic and high-temperature oxidising duty, and 800H/800HT for furnace and cracking temperatures. Metals Fabrica supplies all of these and confirms the alloy, B366 class and heat-treatment condition before quoting.
45°, 90° and 180° long- and short-radius elbows to ASME B16.9 in alloys 600, 625 and 825, formed from seamless or welded nickel-alloy pipe.
Seamless extruded or welded tees for branch connections in high-temperature and corrosive service, ordered by run and branch size and schedule.
Reducers joining two nickel-alloy pipe sizes, with eccentric types used where liquid must drain or vapour must not collect at the top.
MSS SP-43 and ASME B16.9 stub ends that let a carbon or stainless lap-joint flange be used with a nickel-alloy line, plus end caps.
Lighter-wall CR class fittings in schedules 5S and 10S for low-pressure corrosive service, where full B16.9 wall thickness is not needed.
Class 3000 and 6000 elbows, tees, couplings, unions and olets forged from ASTM B564 625 or 825 for small-bore process connections.
| Specification | Details |
|---|---|
| Butt-weld standard | ASTM B366 / ASME SB366: WPNCI (600), WPNCMC (625), WPNIC (800), WPNIC10 (800H), WPNIC11 (800HT), WPNICMC (825) |
| Forged standard | ASTM B564 / ASME SB564 (N06600, N06625, N08800, N08810, N08811, N08825) |
| B366 classes | WP-S, WP-W, WP-WX, WP-WU (ASME B16.9); CR-S, CR-W (MSS SP-43) |
| Starting material | Pipe ASTM B167, B444, B407, B423 (seamless), B517, B705, B514 (welded); plate B168, B443, B409, B424 |
| Dimension standards | ASME B16.9, MSS SP-43, ASME B16.11, MSS SP-97 |
| Size range | 1/2" NB to 48" NB butt-weld; 1/8" to 4" forged |
| Wall thickness | SCH 5S, 10S, 40S, 80S, 160, XXS |
| Heat treatment | Annealed or solution annealed as required by the starting material specification; 800H and 800HT solution annealed for coarse grain |
| Ends | Bevelled to ASME B16.25; socket weld; NPT threaded |
| Testing | Tests of the starting material, dimensional and visual inspection, radiography or UT of welds per class; PMI, IGC and dye penetrant on request |
| Documentation | EN 10204 3.1 certificate; EN 10204 3.2 with third-party inspection on request |
Name the alloy, B366 grade and class, size and schedule in your enquiry. Large welded sizes depend on alloy and plate availability.
| Alloy | UNS | B366 Grade | Ni | Cr | Fe | Mo | C | Mn | Si | S | Other |
|---|---|---|---|---|---|---|---|---|---|---|---|
| Inconel 600 | N06600 | WPNCI | 72.0 min | 14.0 – 17.0 | 6.0 – 10.0 | – | 0.15 | 1.00 | 0.50 | 0.015 | Cu 0.50 |
| Inconel 625 | N06625 | WPNCMC | 58.0 min | 20.0 – 23.0 | 5.0 | 8.0 – 10.0 | 0.10 | 0.50 | 0.50 | 0.015 | Nb+Ta 3.15 – 4.15; Al 0.40; Ti 0.40; P 0.015; Co 1.0 |
| Incoloy 800 | N08800 | WPNIC | 30.0 – 35.0 | 19.0 – 23.0 | 39.5 min | – | 0.10 | 1.50 | 1.00 | 0.015 | Cu 0.75; Al 0.15 – 0.60; Ti 0.15 – 0.60 |
| Incoloy 800H | N08810 | WPNIC10 | 30.0 – 35.0 | 19.0 – 23.0 | 39.5 min | – | 0.05 – 0.10 | 1.50 | 1.00 | 0.015 | Cu 0.75; Al 0.15 – 0.60; Ti 0.15 – 0.60 |
| Incoloy 800HT | N08811 | WPNIC11 | 30.0 – 35.0 | 19.0 – 23.0 | 39.5 min | – | 0.06 – 0.10 | 1.50 | 1.00 | 0.015 | Cu 0.75; Al 0.25 – 0.60; Ti 0.25 – 0.60; Al+Ti 0.85 – 1.20 |
| Incoloy 825 | N08825 | WPNICMC | 38.0 – 46.0 | 19.5 – 23.5 | 22.0 min | 2.5 – 3.5 | 0.05 | 1.0 | 0.5 | 0.03 | Cu 1.5 – 3.0; Ti 0.6 – 1.2; Al 0.2 |
Nickel values include cobalt where the standard says so. Fittings made from plate or bar follow that product's specification, whose limits can differ slightly.
| Alloy | Condition | Tensile Strength, min | Yield Strength (0.2% Offset), min | Elongation, min |
|---|---|---|---|---|
| Inconel 600 | Annealed | 550 MPa (80 ksi) | 240 MPa (35 ksi) | 30% |
| Inconel 625 | Grade 1, annealed | 827 MPa (120 ksi) | 414 MPa (60 ksi) | 30% |
| Inconel 625 | Grade 2, solution annealed | 690 MPa (100 ksi) | 276 MPa (40 ksi) | 30% |
| Incoloy 800 | Annealed | 520 MPa (75 ksi) | 205 MPa (30 ksi) | 30% |
| Incoloy 800H, 800HT | Solution annealed | 450 MPa (65 ksi) | 170 MPa (25 ksi) | 30% |
| Incoloy 825 | Annealed | 586 MPa (85 ksi) | 241 MPa (35 ksi) | 30% |
Requirements vary with product form, size and condition in each starting material specification. 625 Grade 2 is used for service above about 595 °C. Typical densities: 600 8.47, 625 8.44, 800 series 7.94, 825 8.14 g/cm³ (not specification values).
| Alloy | UNS | Werkstoff Nr. | EN | JIS | BS | AFNOR | GOST |
|---|---|---|---|---|---|---|---|
| Inconel 600 | N06600 | 2.4816 | NiCr15Fe | NCF 600 | NA 14 | NC15Fe | – |
| Inconel 625 | N06625 | 2.4856 | NiCr22Mo9Nb | NCF 625 | NA 21 | NC22DNb | – |
| Incoloy 800 | N08800 | 1.4876 | X10NiCrAlTi32-21 | NCF 800 | NA 15 | – | – |
| Incoloy 800H | N08810 | 1.4958 | X5NiCrAlTi31-20 | NCF 800H | NA 15(H) | – | – |
| Incoloy 800HT | N08811 | 1.4959 | X8NiCrAlTi32-21 | – | – | – | – |
| Incoloy 825 | N08825 | 2.4858 | NiCr21Mo | NCF 825 | NA 16 | – | – |
Equivalents are approximate and may differ in some element limits. Order to the ASTM/ASME standard and UNS number in your specification.
Alloy 625 fittings for seawater, firewater and produced-water lines, where molybdenum and niobium give strong resistance to pitting and crevice corrosion.
Incoloy 825 fittings for sulphuric and phosphoric acid service and wet sour gas, where its copper and molybdenum content resist reducing acids.
Incoloy 800H and 800HT fittings in reformer outlet systems, pigtails and ethylene furnace piping that operate above 600 °C.
Inconel 600 fittings for hot caustic soda, chlorine and chloride-bearing streams, where nickel content prevents stress corrosion cracking.
Alloy 625 fittings in scrubber and flue-gas desulphurisation piping exposed to acid condensates and chlorides, where stainless steels suffer pitting and crevice attack.
Alloy 600 and 800 fittings for process gas, muffle and retort piping where oxidation and carburisation resistance are needed at high temperature.
ASTM B366 / ASME SB366 covers factory-made wrought nickel and nickel-alloy fittings. Alloy 600 is grade WPNCI, 625 is WPNCMC and 825 is WPNICMC. Forged socket-weld and threaded fittings are usually made from ASTM B564 forgings.
WP classes follow ASME B16.9 dimensions and pressure ratings, while CR classes follow MSS SP-43 light-wall dimensions. The suffix S means seamless, W welded with radiography of fabrication welds, WX all welds radiographed and WU welds ultrasonically examined.
625 has higher strength and better resistance to pitting in seawater and chlorides. 825 is a lower-cost choice for sulphuric and phosphoric acid and many sour service conditions.
800H and 800HT have controlled carbon and a solution-annealed coarse grain for higher creep strength above about 600 °C. 800HT further restricts aluminium and titanium, while plain 800 is used at lower temperatures.
No. B366 requires the fitting to meet the chemistry and tensile requirements of the pipe, plate or bar specification it is made from, such as B444 or B443 for alloy 625.