EN 10216 is the European product standard for seamless steel tubes used in pressure equipment and pressure piping. It is published in five parts; Parts 1 to 4 cover carbon, carbon-manganese and ferritic alloy steels, and Part 5 covers stainless steels. Each part sets chemical composition, tensile properties, impact energy, heat treatment, test category and inspection documents, while outside diameter and wall thickness follow EN 10220.
Part 1 covers non-alloy steels with specified room-temperature properties, P195, P235 and P265, each in TR1 (no impact test or aluminium requirement) or TR2 (impact tested, aluminium killed). Part 2 covers steels with specified elevated-temperature properties, from carbon grades such as P235GH and P265GH to molybdenum and chromium-molybdenum grades such as 16Mo3, 13CrMo4-5, 10CrMo9-10 and X10CrMoVNb9-1. Part 3 covers normalised fine-grain steels such as P355N and P460N, and Part 4 covers steels with specified low-temperature toughness, from P265NL to 9% nickel X10Ni9.
Choose the part by design condition: Part 1 for ambient utility and process lines, Part 2 when the design uses elevated-temperature proof strength, Part 3 for higher strength at moderate temperature and Part 4 for sub-zero service. Test category TC1 or TC2 sets the extent of NDT and leak testing. For welded equivalents of Part 1 grades, see EN 10217-1 P235TR1 pipe. Metals Fabrica identifies which EN 10216 part your grade belongs to and confirms the test category and inspection document, 3.1 or 3.2, before quoting.
Non-alloy tube with room-temperature properties; TR2 adds aluminium-killed steel, impact testing and tighter limits for pressure equipment needing traceable toughness.
Carbon steel boiler and pressure tube with specified 0.2% proof strength at elevated temperature, used for feedwater, steam and header lines.
Molybdenum and chromium-molybdenum tubes for superheaters and steam piping where creep strength and oxidation resistance above carbon-steel limits are needed.
2.25Cr-1Mo and 9Cr-1Mo-V grades for high-pressure, high-temperature power-plant lines, offering higher creep rupture strength than lower-alloy grades at the same wall thickness.
Normalised fine-grain P275NL1, P355N and P460N grades offering higher yield strength with good weldability for vessels and hydraulic lines.
P265NL, 12Ni14 and X10Ni9 grades with impact energy guaranteed at sub-zero temperatures for refrigeration, LPG and cryogenic duty.
| Specification | Details |
|---|---|
| Product standard | EN 10216-1, EN 10216-2, EN 10216-3, EN 10216-4 (seamless tubes for pressure purposes) |
| Related ASME / ASTM | Nearest: ASTM A106, A179, A192, A333, A335 (approximate, not interchangeable) |
| Dimension standard | EN 10220 |
| Size range | 10.2 mm to 914 mm OD |
| Wall thickness | 1.0 mm to 60 mm and to order |
| Manufacturing type | Seamless, hot finished or cold finished |
| Heat treatment | Normalised or normalising formed (non-alloy); normalised and tempered or quenched and tempered (alloy grades) |
| Test category | TC1 or TC2 per part; TC2 includes NDT for longitudinal imperfections |
| Ends | Plain end, bevelled end |
| Length | Random and fixed lengths |
| Testing | Tensile, flattening or ring tests, impact (where specified), leak tightness, NDT, dimensional and visual inspection |
| Documentation | EN 10204 3.1 inspection certificate; EN 10204 3.2 on request |
Name the part, grade, test category and any options in your enquiry. ERW and SAW tubes fall under EN 10217, not EN 10216.
| Grade | Part | C | Si | Mn | P | S | Cr | Mo | Other |
|---|---|---|---|---|---|---|---|---|---|
| P195TR1 / TR2 | -1 | 0.13 | 0.35 | 0.70 | 0.025 | 0.020 / 0.015 | 0.30 | 0.08 | Ni 0.30; Cu 0.30 |
| P235TR1 / TR2 | -1 | 0.16 | 0.35 | 1.20 | 0.025 | 0.020 / 0.015 | 0.30 | 0.08 | Ni 0.30; Cu 0.30 |
| P265TR1 / TR2 | -1 | 0.20 | 0.40 | 1.40 | 0.025 | 0.020 / 0.015 | 0.30 | 0.08 | Ni 0.30; Cu 0.30 |
| P235GH | -2 | 0.16 | 0.35 | 1.20 | 0.025 | 0.020 | 0.30 | 0.08 | Al 0.020 min; Ni 0.30; Cu 0.30 |
| P265GH | -2 | 0.20 | 0.40 | 1.40 | 0.025 | 0.020 | 0.30 | 0.08 | Al 0.020 min; Ni 0.30; Cu 0.30 |
| 16Mo3 | -2 | 0.12 – 0.20 | 0.35 | 0.40 – 0.90 | 0.025 | 0.020 | 0.30 | 0.25 – 0.35 | Ni 0.30; Cu 0.30 |
| 13CrMo4-5 | -2 | 0.10 – 0.17 | 0.35 | 0.40 – 0.70 | 0.025 | 0.020 | 0.70 – 1.15 | 0.40 – 0.60 | Ni 0.30; Cu 0.30 |
| 10CrMo9-10 | -2 | 0.08 – 0.14 | 0.50 | 0.30 – 0.70 | 0.025 | 0.020 | 2.00 – 2.50 | 0.90 – 1.10 | Ni 0.30; Cu 0.30 |
| X10CrMoVNb9-1 | -2 | 0.08 – 0.12 | 0.20 – 0.50 | 0.30 – 0.60 | 0.020 | 0.010 | 8.00 – 9.50 | 0.85 – 1.05 | V 0.18 – 0.25; Nb 0.06 – 0.10; N 0.030 – 0.070; Ni 0.40 |
Weight %, maximum unless a range or minimum is shown. Where two S values are given, the first is TR1 and the second TR2.
| Grade | Part | C | Si | Mn | P | S | Ni | Other |
|---|---|---|---|---|---|---|---|---|
| P355N | -3 | 0.20 | 0.50 | 0.90 – 1.70 | 0.025 | 0.020 | 0.50 | Al 0.020 min; Nb, V, Ti limits apply |
| P265NL | -4 | 0.20 | 0.40 | 0.60 – 1.40 | 0.025 | 0.020 | 0.30 | Al 0.020 min |
| 12Ni14 | -4 | 0.15 | 0.35 | 0.30 – 0.80 | 0.025 | 0.010 | 3.25 – 3.75 | – |
| X10Ni9 | -4 | 0.10 | 0.35 | 0.30 – 0.80 | 0.020 | 0.010 | 8.50 – 10.00 | – |
Weight %, maximum unless a range or minimum is shown. Values summarised for comparison; residual element limits are given in each part.
| Grade | Part | Yield Strength ReH, min | Tensile Strength Rm | Elongation A, min (long. / trans.) |
|---|---|---|---|---|
| P195TR1 / TR2 | -1 | 195 MPa | 320 – 440 MPa | 27% / 25% |
| P235TR1 / TR2 | -1 | 235 MPa | 360 – 500 MPa | 25% / 23% |
| P265TR1 / TR2 | -1 | 265 MPa | 410 – 570 MPa | 21% / 19% |
| P235GH | -2 | 235 MPa | 360 – 500 MPa | 25% / 23% |
| P265GH | -2 | 265 MPa | 410 – 570 MPa | 23% / 21% |
| 16Mo3 | -2 | 280 MPa | 450 – 600 MPa | 22% / 20% |
| 13CrMo4-5 | -2 | 290 MPa | 440 – 590 MPa | 22% / 20% |
| 10CrMo9-10 | -2 | 280 MPa | 480 – 630 MPa | 22% / 20% |
| X10CrMoVNb9-1 | -2 | 450 MPa | 630 – 830 MPa | 19% / 17% |
| P355N | -3 | 355 MPa | 490 – 650 MPa | 22% / 20% |
| P265NL | -4 | 265 MPa | 410 – 570 MPa | 24% / 22% |
Impact energy requirements (TR2, Part 2, Part 3 and Part 4 grades) and elevated-temperature proof strength values are given in each part. Density of these steels is typically 7.85 g/cm³.
| Grade | Material No. | ASTM | JIS | BS | GB |
|---|---|---|---|---|---|
| P235TR2 | 1.0255 | A106 Grade A (approx.) | STPG 370 | BS 3601 360 | 10 |
| P235GH | 1.0345 | A106 Grade A / A192 | STPT 370 | BS 3602 HFS 360 | – |
| P265GH | 1.0425 | A106 Grade B | STPT 410 | BS 3602 HFS 410 | 20G |
| 16Mo3 | 1.5415 | A335 P1 | STPA 12 | – | 15MoG |
| 13CrMo4-5 | 1.7335 | A335 P11 / P12 | STPA 22 / STPA 23 | BS 3604 620-440 | 15CrMoG |
| 10CrMo9-10 | 1.7380 | A335 P22 | STPA 24 | BS 3604 622 | 12Cr2MoG |
| X10CrMoVNb9-1 | 1.4903 | A335 P91 | STPA 28 | – | 10Cr9Mo1VNbN |
| P265NL | 1.0453 | A333 Grade 6 (approx.) | STPL 380 | BS 3603 430LT | 16MnDG (approx.) |
Equivalents are approximate. Elevated-temperature strength, impact temperature and testing differ between systems; order to the standard required by your pressure code.
P235GH, P265GH and 16Mo3 tubes for economisers, evaporators and headers designed with the elevated-temperature proof strength values of EN 10216-2.
13CrMo4-5, 10CrMo9-10 and X10CrMoVNb9-1 tubes for high-temperature steam in power and process plants, where long-term creep rupture strength governs the required wall thickness.
Part 1 and Part 3 grades used for nozzles, shell tubes and exchanger bundles in process plants built to EN 13445.
EN 10216-4 P265NL and nickel steels with guaranteed impact energy at low temperatures for ammonia, LPG and ethylene service.
Fine-grain P355N and P460N tubes giving higher allowable stress, which allows thinner, lighter walls in high-pressure hydraulic and compressed-air systems.
P235TR1 and P235TR2 tube for water, air and process lines at ambient temperature, with TR2 chosen when impact testing is required.
EN 10216-1 tubes have specified room-temperature properties only. EN 10216-2 tubes also have specified 0.2% proof strength at elevated temperatures, and include molybdenum and chromium-molybdenum grades, so they are used where the design temperature is above ambient.
TR1 grades have no aluminium or impact energy requirements. TR2 grades are aluminium killed, have tighter limits on some elements and must meet impact energy requirements, which makes them suitable where pressure codes ask for proven toughness.
The test category sets the extent of inspection. TC2 adds non-destructive testing for longitudinal imperfections and other checks to the TC1 programme, and is usually required for more critical pressure equipment.
P265GH is usually compared with ASTM A106 Grade B, since both are carbon steel pressure grades with similar strength. The tensile and yield requirements and elevated-temperature data differ, so they are not automatically interchangeable.
EN 10216-4 covers non-alloy and alloy steel tubes with specified low-temperature properties, such as P265NL, 12Ni14 and X10Ni9. Each grade has a minimum impact energy at a defined sub-zero test temperature.
Outside diameters and wall thicknesses follow EN 10220, which lists preferred series for seamless and welded steel tubes. Tolerances on OD and wall are set in EN 10216 itself.