Copper nickel 70/30 bar is a cupronickel with 29.0–33.0% nickel, 0.40–1.0% iron and up to 1.0% manganese, the balance copper. The high nickel content gives it the best seawater corrosion and erosion resistance of the common copper nickels, and it tolerates higher flow velocities, sulphide-polluted water and hotter brine than the 90/10 grade. ASTM B151 designates it UNS C71500.
Against copper nickel 90/10 bar, 70/30 is noticeably stronger in the annealed condition and harder wearing, which suits it to valve stems, pump parts and fasteners that see turbulence or impingement. It costs more because of the extra nickel, and its antifouling behaviour is slightly weaker than 90/10. Like all copper nickels, it is a single-phase alloy, strengthened only by cold drawing and softened by annealing.
Bar is extruded or hot rolled, then supplied annealed or cold drawn to the tempers listed in B151, with the surface peeled, turned or ground for machining. Metals Fabrica supplies 70/30 bar with temper, size and tolerance confirmed against your drawing, and can quote matching copper nickel 70/30 pipe for the same system.
Soft-annealed C71500 rounds with the highest ductility, used for parts that are formed, upset or heavily machined before installation in seawater.
Drawn to a harder temper and close tolerance for valve stems, shafts and fasteners that need extra strength without heat treatment.
Peeled, then centreless ground to size and straightness, for pump shafts and turned components that leave only a minimal machining allowance.
Hexagon sections for nuts, unions and fittings in condenser and seawater systems, ordered by size across flats and length.
Flat, rectangular and square sections for marine hardware, wear strips and machined brackets exposed to seawater spray or immersion.
| Specification | Details |
|---|---|
| Bar standard | ASTM B151 / ASME SB151 |
| UNS / grade | UNS C71500 (CuNi 70/30) |
| European standard | EN 12163 CW354H (CuNi30Mn1Fe) when named on the order |
| Shapes | Round, hex, square, flat, rectangular |
| Size range | 3 mm to 500 mm round; hex and square to order |
| Length | 1 to 6 m random, fixed and cut lengths |
| Temper | Annealed or cold-drawn tempers as listed in ASTM B151 |
| Finish | Black, bright, peeled, turned, centreless ground |
| Tolerance | Per ASTM B151; h9, h11 or k12 on request |
| Testing | Tensile, chemical analysis, PMI; hardness and ultrasonic testing on request |
| Documentation | EN 10204 3.1 mill test certificate; EN 10204 3.2 on request |
Confirm the temper, size and tolerance in your enquiry.
| Grade | UNS | Cu | Ni (incl. Co) | Fe | Mn | Pb | Zn |
|---|---|---|---|---|---|---|---|
| CuNi 70/30 | C71500 | Remainder | 29.0 – 33.0 | 0.40 – 1.0 | 1.0 | 0.05 | 1.0 |
Cu includes Ag.
| Grade and Temper | Density | Melting Range | Tensile Strength, min | Yield Strength, min |
|---|---|---|---|---|
| CuNi 70/30 (C71500), annealed | 8.95 g/cm³ | 1170 – 1240 °C | 345 MPa (50 ksi) | 125 MPa (18 ksi) |
Density and melting range are typical values, not specification requirements. Drawn tempers have higher, diameter-dependent minimums in ASTM B151.
| Grade | UNS | Werkstoff Nr. | EN / DIN | JIS | BS |
|---|---|---|---|---|---|
| CuNi 70/30 | C71500 | 2.0882 | CuNi30Mn1Fe (CW354H) | C7150 | CN107 |
Equivalents are approximate; iron and manganese ranges differ between standards. Order to the standard named in your specification.
Valve stems, pump parts and fittings for warship cooling and firemain systems, where 70/30 handles high flow velocities and shock loads.
Machined components and fixings for seawater-cooled condensers, especially at coastal sites where the water is polluted or turbulence causes impingement attack.
Parts in the hottest stages of thermal desalination plants, where 70/30 resists brine at higher temperatures than 90/10.
Impeller fixings, stems and seats for seawater lift and injection pumps that combine erosion resistance with moderate strength.
Cold-drawn 70/30 bolts and studs for seawater flanges and hull fittings, chosen for strength and compatibility with copper nickel piping.
Choose 70/30 where parts face high water velocity, turbulence, polluted seawater or hot brine, or where higher strength is needed. For general seawater service at moderate velocity, 90/10 is usually adequate and more economical.
70/30 copper nickel is UNS C71500. The DIN / EN equivalents are 2.0882 and CW354H (CuNi30Mn1Fe).
With iron below 1.0%, 70/30 copper nickel is essentially non-magnetic in normal use, although very slight magnetic response can occur with higher iron levels.
Only by cold drawing. The alloy is not heat treatable, so drawn tempers have higher strength than annealed bar, and annealing restores full ductility.