ASTM A234 WP11 fittings are made from 1¼% chromium, ½% molybdenum steel and are the most widely used chrome-moly fittings. They pair with ASTM A335 P11 pipe in steam lines, boiler headers and refinery units operating at roughly 400 to 550 °C, where carbon steel loses creep strength.
WP11 is the only A234 grade ordered in three classes, and the classes differ in chemistry as well as strength. Class 1 has tighter limits (carbon 0.05–0.15%, manganese 0.30–0.60%, phosphorus and sulphur 0.030% max) and a tensile range of 415–585 MPa. Classes 2 and 3 allow carbon up to 0.20% and manganese up to 0.80%, and must reach 485–655 MPa and 520–690 MPa respectively. Silicon of 0.50–1.00% is required in every class and helps oxidation resistance. Fittings are normalised and tempered after forming.
WP11 has lower creep strength than WP22, so it is usually chosen for the cooler end of the temperature range. Metals Fabrica supplies WP11 fittings and checks that the class on the certificate matches the pipe class in your line specification, since Class 1 and Class 2 material are often confused.
Lower-carbon WP11 with 415 to 585 MPa tensile, favoured for weldability and specified with A335 P11 in many power and refinery line classes.
Higher carbon and manganese limits give 485 to 655 MPa tensile and 275 MPa yield, for designs needing more strength than Class 1.
The strongest WP11 class at 520 to 690 MPa tensile and 310 MPa yield, used where the line design is based on higher allowable stresses.
45°, 90° and 180° long- and short-radius elbows to ASME B16.9, hot formed from P11 pipe and normalised and tempered after forming.
Equal and reducing tees, concentric and eccentric reducers, and caps in the schedule of the connecting P11 pipe for headers and branches.
Socket-weld and threaded elbows, tees, couplings, unions and olets to ASME B16.11 and MSS SP-97 for small-bore steam drains and vents.
| Specification | Details |
|---|---|
| Standard / grade | ASTM A234 / ASME SA234 WP11 Class 1, Class 2, Class 3 |
| Forged fittings | ASTM A182 / ASME SA182 F11 Class 1, 2, 3 |
| Dimension standards | ASME B16.9, ASME B16.11, MSS SP-97, MSS SP-79, MSS SP-83 |
| Size range | 1/2" NB to 48" NB butt-weld; 1/8" to 4" forged |
| Wall thickness | SCH 10 to SCH 160, STD, XS, XXS, to match the pipe |
| Construction | Seamless or welded (marked W); forged socket-weld and threaded |
| Heat treatment | Normalised and tempered, or annealed, per ASTM A234 |
| Hardness | 197 HBW max (Class 1); 217 HBW max (Class 2 and 3) |
| Ends | Bevelled to ASME B16.25; socket weld; NPT threaded |
| Testing | Tensile and hardness tests, dimensional and visual inspection, radiography of welds; PMI and MPI on request |
| Documentation | EN 10204 3.1 certificate; EN 10204 3.2 on request |
Always state the class. WP11 without a class is not a complete designation under current editions of A234.
| Grade | C | Mn | P | S | Si | Cr | Mo |
|---|---|---|---|---|---|---|---|
| WP11 Class 1 | 0.05 – 0.15 | 0.30 – 0.60 | 0.030 | 0.030 | 0.50 – 1.00 | 1.00 – 1.50 | 0.44 – 0.65 |
| WP11 Class 2, Class 3 | 0.05 – 0.20 | 0.30 – 0.80 | 0.040 | 0.040 | 0.50 – 1.00 | 1.00 – 1.50 | 0.44 – 0.65 |
| Grade | Tensile Strength | Yield Strength, min | Elongation, min (longitudinal) | Hardness, max | Density |
|---|---|---|---|---|---|
| WP11 Class 1 | 415 – 585 MPa (60 – 85 ksi) | 205 MPa (30 ksi) | 22% | 197 HBW | 7.85 g/cm³ |
| WP11 Class 2 | 485 – 655 MPa (70 – 95 ksi) | 275 MPa (40 ksi) | 22% | 217 HBW | 7.85 g/cm³ |
| WP11 Class 3 | 520 – 690 MPa (75 – 100 ksi) | 310 MPa (45 ksi) | 22% | 217 HBW | 7.85 g/cm³ |
Density is a typical value, not a specification requirement. Elongation is for a standard round specimen in 4D.
| Fitting Grade (A234) | Pipe (A335) | Forging (A182) | Plate | EN (Material No.) | JIS (pipe) | GB (pipe) |
|---|---|---|---|---|---|---|
| WP11 Class 1 | P11 | F11 Class 1 | A387 Gr 11 Class 1 | 13CrMo4-5 (1.7335) | STPA 23 | – |
| WP11 Class 2, 3 | P11 | F11 Class 2, 3 | A387 Gr 11 Class 2 | 13CrMo4-5 (1.7335) | STPA 23 | – |
13CrMo4-5 has lower silicon and is closer to the 1Cr-½Mo P12 grade; it is an approximate equivalent only. Order to the standard in your specification.
Header, link and drain fittings in utility and industrial boilers, where WP11 handles steam temperatures beyond the creep limit of carbon steel.
Reactor feed and effluent piping where 1¼Cr-½Mo provides resistance to high-temperature hydrogen attack at moderate temperatures and pressures.
FCC reactor and regenerator piping, steam lines and transfer piping operating in the 400 to 500 °C range.
Fittings for the cooler pressure sections of heat recovery steam generators, alongside WP22 and WP91 in the hotter zones.
High-pressure steam distribution in chemical, fertiliser and paper plants where temperatures call for chrome-moly rather than carbon steel.
Class 1 has tighter carbon, manganese, phosphorus and sulphur limits and requires 415–585 MPa tensile. Class 2 and Class 3 allow up to 0.20% carbon and 0.80% manganese and require 485–655 MPa and 520–690 MPa respectively.
Yes, the class is chosen for the design strength, and the piping specification states which class is acceptable. Class 2 fittings are often used where the fitting must at least match the strength of the pipe.
Allowable stresses for 1¼Cr-½Mo are listed in ASME B31.1, B31.3 and Section II Part D up to well above 550 °C, but creep strength falls quickly at the upper end. WP22 or WP91 is usually chosen for higher steam temperatures.
No. WP12 is a 1Cr-½Mo grade with lower silicon, matching A335 P12 pipe. WP11 has 1.00–1.50% chromium and 0.50–1.00% silicon and matches P11.
ASTM A182 F11 is the matching forging grade, supplied in Class 1, 2 or 3 to suit the butt-weld fitting class.