ASTM A234 WP22 fittings are made from 2¼% chromium, 1% molybdenum steel, the workhorse alloy for high-temperature steam and high-pressure hydrogen piping. They are used with ASTM A335 P22 pipe in main steam and hot reheat lines, boiler headers and hydrocracker reactor circuits.
The higher molybdenum content (0.87–1.13%) gives WP22 noticeably better creep-rupture strength than WP11 at temperatures above about 480 °C, which allows thinner walls for the same design conditions. Unlike WP11, WP22 limits silicon to 0.50% max. It is supplied in two classes with one chemistry: Class 1 at 415–585 MPa tensile and 205 MPa yield, and Class 3 at 520–690 MPa tensile and 310 MPa yield. Fittings are normalised and tempered, and hardness is limited to 217 HBW.
For supercritical boilers and the hottest steam lines, WP22 is increasingly replaced by WP91, which carries much higher allowable stresses. WP22 remains the usual choice for hydrogen service because its behaviour under API 941 is well documented. Metals Fabrica supplies WP22 fittings with the class, heat treatment and hardness confirmed against your line specification.
The standard WP22 strength level, 415 to 585 MPa tensile and 205 MPa yield, matching A335 P22 pipe in most power and refinery specifications.
Same 2¼Cr-1Mo chemistry heat treated to 520 to 690 MPa tensile and 310 MPa yield, for heavy-wall and high-pressure designs.
90° and 45° long-radius elbows to ASME B16.9 for main steam and hot reheat routing, often in heavy schedules or specified minimum wall.
Extruded or hot-pressed tees for steam headers and reactor piping, with crotch reinforcement sized for the run pipe pressure.
Concentric and eccentric reducers and butt-weld caps for size transitions, header ends and dead legs in 2¼Cr-1Mo steam and process lines.
Socket-weld and threaded fittings and olets in Class 3000, 6000 and 9000 forged from A182 F22 for drains, vents and instrument tappings.
| Specification | Details |
|---|---|
| Standard / grade | ASTM A234 / ASME SA234 WP22 Class 1, WP22 Class 3 |
| Forged fittings | ASTM A182 / ASME SA182 F22 Class 1, Class 3 |
| Dimension standards | ASME B16.9, ASME B16.11, MSS SP-97 |
| Size range | 1/2" NB to 48" NB butt-weld; 1/8" to 4" forged |
| Wall thickness | SCH 10 to SCH 160, STD, XS, XXS, or minimum wall to match the pipe |
| Construction | Seamless or welded (marked W); forged socket-weld and threaded |
| Heat treatment | Normalised and tempered, or annealed, per ASTM A234 |
| Hardness | 217 HBW max |
| Ends | Bevelled to ASME B16.25; socket weld; NPT threaded |
| Testing | Tensile and hardness tests, dimensional and visual inspection, radiography of welds; UT, MPI and PMI on request |
| Documentation | EN 10204 3.1 certificate; EN 10204 3.2 on request |
For hydrogen service, include any additional hardness, toughness or step-cooling requirements from your project specification.
| Grade | C | Mn | P | S | Si | Cr | Mo |
|---|---|---|---|---|---|---|---|
| WP22 Class 1, Class 3 | 0.05 – 0.15 | 0.30 – 0.60 | 0.040 | 0.040 | 0.50 | 1.90 – 2.60 | 0.87 – 1.13 |
| Grade | Tensile Strength | Yield Strength, min | Elongation, min (longitudinal) | Hardness, max | Density |
|---|---|---|---|---|---|
| WP22 Class 1 | 415 – 585 MPa (60 – 85 ksi) | 205 MPa (30 ksi) | 22% | 217 HBW | 7.83 g/cm³ |
| WP22 Class 3 | 520 – 690 MPa (75 – 100 ksi) | 310 MPa (45 ksi) | 22% | 217 HBW | 7.83 g/cm³ |
Density is a typical value, not a specification requirement. Elongation is for a standard round specimen in 4D.
| Fitting Grade (A234) | Pipe (A335) | Forging (A182) | Plate | EN (Material No.) | JIS (pipe) | GB (pipe) |
|---|---|---|---|---|---|---|
| WP22 Class 1 | P22 | F22 Class 1 | A387 Gr 22 Class 1 | 10CrMo9-10 (1.7380) | STPA 24 | 12Cr2MoG |
| WP22 Class 3 | P22 | F22 Class 3 | A387 Gr 22 Class 2 | 10CrMo9-10 (1.7380) | STPA 24 | 12Cr2MoG |
Equivalents are close 2¼Cr-1Mo steels with differing strength requirements. Order to the standard in your specification.
Elbows and tees in subcritical power plant steam piping, where 2¼Cr-1Mo creep strength supports long service at 540 °C and above.
High-pressure hydrogen and hydrocarbon lines around hydrocracker reactors, where WP22 is selected for its documented resistance to high-temperature hydrogen attack.
Header end caps, branch tees and link pipe fittings in superheater and reheater sections of utility and industrial boilers.
Hot transfer piping from heaters to reactors and fractionators, where temperature and pressure exceed the economic range of WP11.
High-pressure superheater and steam outlet fittings in heat recovery steam generators, usually installed alongside WP91 components in the hottest sections.
Both have the same 2¼Cr-1Mo chemistry. Class 1 requires 415–585 MPa tensile and 205 MPa yield; Class 3 requires 520–690 MPa tensile and 310 MPa yield, achieved by heat treatment.
ASTM A234 lists WP22 only in Class 1 and Class 3. The class numbers align the fitting strength levels with those of other A234 chrome-moly grades rather than forming a continuous series.
WP91 has much higher allowable stress at 550–600 °C, so it allows thinner walls in supercritical and high-temperature designs. WP22 remains common in subcritical plants and hydrogen service, and is easier to weld and heat treat.
WP22 fittings are used with ASTM A335 P22 pipe and ASTM A182 F22 flanges and forged fittings, in the class required by the piping specification.
ASTM A234 limits WP22 fittings to 217 HBW. Hydrogen and sour-service specifications often impose a lower limit, which should be stated in the enquiry.