ASTM A234 WP91 fittings are made from modified 9Cr-1Mo steel, a creep-strength-enhanced ferritic (CSEF) alloy. Small, controlled additions of vanadium, niobium and nitrogen form fine carbonitride precipitates in a tempered martensite structure, giving creep strength far above conventional chrome-moly. This allows thinner, lighter fittings with ASTM A335 P91 pipe in supercritical and combined-cycle steam systems running at 565 to 600 °C.
WP91 has a minimum yield of 415 MPa and tensile of 585–760 MPa, about double the yield of WP22 Class 1 fittings. Its properties depend almost entirely on correct heat treatment: fittings are normalised and then tempered within a narrow window, and both under- and over-tempering reduce creep life. Current editions of A234 recognise Type 1 and Type 2. Type 2 tightens manganese, silicon, sulphur and nickel and adds limits on copper, boron, tungsten, titanium, zirconium and tramp elements such as arsenic, tin and antimony, plus a minimum nitrogen-to-aluminium ratio.
Because WP91 is unforgiving of welding and PWHT errors, buyers usually specify hardness checks on every fitting and PMI for chromium, molybdenum and vanadium. Metals Fabrica supplies WP91 fittings with the type, heat-treatment temperatures and hardness results confirmed on the certificate before dispatch.
The original modified 9Cr-1Mo chemistry, still accepted by many power plant specifications and matching A335 P91 Type 1 pipe.
Tighter chemistry with limits on residual and tramp elements and a minimum N/Al ratio, specified by owners seeking more consistent creep performance.
Hot-formed 90° and 45° elbows for main steam and hot reheat routing, renormalised and tempered after forming and hardness tested.
Extruded and hot-pressed equal and reducing tees for steam headers and turbine bypass lines, in heavy wall or minimum wall to match P91.
Concentric and eccentric reducers and end caps for HRSG headers and steam lines, supplied with full heat-treatment records.
Socket-weld fittings, weldolets and sockolets forged from A182 F91 for drains, vents and instrument branches on P91 headers.
| Specification | Details |
|---|---|
| Standard / grade | ASTM A234 / ASME SA234 WP91 Type 1, WP91 Type 2 |
| Forged fittings | ASTM A182 / ASME SA182 F91 |
| Dimension standards | ASME B16.9, ASME B16.11, MSS SP-97 |
| Size range | 1/2" NB to 48" NB butt-weld; 1/8" to 4" forged |
| Wall thickness | SCH 40 to SCH 160, XS, XXS, or minimum wall to match the pipe |
| Construction | Seamless or welded (marked W); forged socket-weld |
| Heat treatment | Normalised at 1040 – 1080 °C and tempered at 730 – 800 °C |
| Hardness | 248 HBW max; many project specifications also set a minimum |
| Ends | Bevelled to ASME B16.25; socket weld |
| Testing | Tensile and hardness test, dimensional and visual inspection, radiography of welds; PMI, UT and hardness on each fitting on request |
| Documentation | EN 10204 3.1 certificate with heat-treatment temperatures; EN 10204 3.2 on request |
State Type 1 or Type 2 and any project hardness range in your enquiry.
| Grade | C | Mn | P | S | Si | Cr | Mo | Ni | V | Nb | N | Al | Other |
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| WP91 Type 1 | 0.08 – 0.12 | 0.30 – 0.60 | 0.020 | 0.010 | 0.20 – 0.50 | 8.0 – 9.5 | 0.85 – 1.05 | 0.40 | 0.18 – 0.25 | 0.06 – 0.10 | 0.030 – 0.070 | 0.02 | Ti 0.01; Zr 0.01 |
| WP91 Type 2 | 0.08 – 0.12 | 0.30 – 0.50 | 0.020 | 0.005 | 0.20 – 0.40 | 8.0 – 9.5 | 0.85 – 1.05 | 0.20 | 0.18 – 0.25 | 0.06 – 0.10 | 0.035 – 0.070 | 0.020 | Cu 0.10; B 0.001; W 0.05; Ti 0.01; Zr 0.01; As 0.010; Sn 0.010; Sb 0.003; N/Al ≥ 4.0 |
| Grade | Tensile Strength | Yield Strength, min | Elongation, min (longitudinal) | Hardness, max | Density |
|---|---|---|---|---|---|
| WP91 Type 1, Type 2 | 585 – 760 MPa (85 – 110 ksi) | 415 MPa (60 ksi) | 20% | 248 HBW | 7.77 g/cm³ |
Density is a typical value, not a specification requirement. Elongation is for a standard round specimen in 4D. Project specifications commonly require a hardness window rather than a maximum only.
| Fitting Grade (A234) | Pipe (A335) | Forging (A182) | Plate | EN (Material No.) | JIS (pipe) | GB (pipe) |
|---|---|---|---|---|---|---|
| WP91 | P91 | F91 | A387 Gr 91 | X10CrMoVNb9-1 (1.4903) | STPA 28 | 10Cr9Mo1VNbN |
These are the closest modified 9Cr-1Mo grades; residual-element and heat-treatment limits differ, especially against WP91 Type 2.
Elbows and tees in main steam and hot reheat lines of supercritical units, where WP91 creep strength keeps wall thickness and thermal stress manageable.
Superheater and reheater header fittings in combined-cycle plants that start and stop daily, where thinner walls reduce thermal fatigue damage.
High-temperature steam leads and bypass piping near turbines, where space, support and nozzle load limits favour lighter P91 components.
Selected furnace and heater piping where 9Cr-1Mo-V offers higher strength than WP9 at the same metal temperature, allowing lighter coil and header designs.
Type 2 narrows the limits on manganese, silicon, sulphur and nickel, raises the minimum nitrogen, and adds maximums for copper, boron, tungsten and tramp elements with a minimum N/Al ratio of 4.0. Tensile requirements are the same for both types.
WP91 creep strength depends on correct normalising and tempering. Hardness that is too high indicates under-tempering; hardness that is too low suggests over-tempering or incorrect normalising, both of which shorten creep life.
Dissimilar welds between P91 and P22 are made in power plants, but they need a qualified procedure, suitable filler metal and PWHT chosen to suit both materials. Matching WP91 to P91 pipe is normally preferred.
ASTM A234 requires normalising at 1040–1080 °C followed by tempering at 730–800 °C. Project specifications often narrow the tempering range further.