Monel K500 bar is the precipitation-hardenable version of the nickel-copper alloy. It keeps the 63% minimum nickel and roughly 30% copper of Monel 400, adding 2.30–3.15% aluminium and 0.35–0.85% titanium. During ageing these elements precipitate as fine gamma-prime particles, Ni3(Al,Ti), which lift yield strength to about three or four times that of annealed 400 while corrosion behaviour in seawater and alkalis stays much the same.
ASTM B865 recognises several delivery conditions. Bar can be supplied solution annealed (soft, for machining and forming), or aged after hot finishing, after annealing, or after cold drawing. A typical age is around 590–610 °C for up to 16 hours followed by slow furnace cooling to about 480 °C; the exact cycle depends on prior cold work. Aged bar is hard and machines more slowly, so complex parts are often roughed in the annealed condition and aged afterwards.
Choose K500 over Monel 400 bar for pump shafts, impellers, springs, high-strength fasteners and non-magnetic drill collars. Metals Fabrica supplies K500 bar in the condition specified on your order and checks whether the ageing is to be done before or after your machining. For tubular parts, see Monel K500 pipe.
Soft bar for parts that are heavily machined, upset or formed first and aged afterwards, keeping tool wear and distortion of the finished part low.
Hot rolled or forged, then aged to high strength. Commonly ordered for pump and propeller shafts in larger diameters.
Annealed and then aged, giving slightly lower strength than hot-finished and aged bar but more uniform properties through the section.
Cold drawing before ageing gives the highest strength levels in B865, suited to small-diameter fasteners, springs and precision shafts.
Aged bar ground to tight diameter tolerance and straightness for pump and impeller shafts that need minimal finish machining.
Hexagon bar, usually aged, for high-strength nuts, bolts and fittings used in seawater, sour oil and gas, and chemical service.
| Specification | Details |
|---|---|
| Bar standard | ASTM B865 |
| UNS / grade | UNS N05500 (Alloy K-500) |
| Other specifications | QQ-N-286, AMS 4676, NACE MR0175 / ISO 15156 hardness limits when named on the order |
| Shapes | Round, hex, square, flat, rectangular; forged blocks |
| Size range | 3 mm to 500 mm round; hex and square to order |
| Length | 1 to 6 m random, fixed and cut lengths |
| Condition | Solution annealed; hot finished and aged; annealed and aged; cold drawn and aged |
| Finish | Black, bright, peeled, turned, centreless ground, polished |
| Tolerance | Per ASTM B865; h9, h11 or k12 on request |
| Testing | Tensile and hardness in the delivered condition, chemical analysis, PMI; ultrasonic testing on request |
| Documentation | EN 10204 3.1 certificate stating condition and ageing; EN 10204 3.2 on request |
State the delivery condition clearly. Aged bar and annealed bar intended for later ageing are different products.
| Grade | UNS | Ni (incl. Co) | Cu | Al | Ti | Fe | Mn | C | Si | S |
|---|---|---|---|---|---|---|---|---|---|---|
| Monel K500 | N05500 | 63.0 min | 27.0 – 33.0 | 2.30 – 3.15 | 0.35 – 0.85 | 2.0 | 1.5 | 0.25 | 0.5 | 0.01 |
| Condition | Tensile Strength, min | Yield Strength (0.2% Offset), min | Elongation in 50 mm or 4D, min |
|---|---|---|---|
| Hot finished and aged | 965 MPa (140 ksi) | 690 MPa (100 ksi) | 20% |
| Annealed and aged | 895 MPa (130 ksi) | 585 MPa (85 ksi) | 20% |
| Cold drawn and aged | 965 MPa (140 ksi) | 690 MPa (100 ksi) | 17% |
Minimums depend on diameter; larger sizes have lower values in ASTM B865. Check the size limits for your diameter in the current edition.
| Condition | Density | Melting Range | Tensile Strength | Yield Strength (0.2% Offset) | Hardness |
|---|---|---|---|---|---|
| Solution annealed | 8.44 g/cm³ | 1315 – 1350 °C | approx. 620 – 760 MPa (90 – 110 ksi) | approx. 275 – 415 MPa (40 – 60 ksi) | approx. 75 – 90 HRB |
Typical values for information, not specification minimums. Annealed bar reaches the aged properties only after the specified ageing treatment.
| Grade | UNS | Werkstoff Nr. | EN | JIS | BS | AFNOR | GOST |
|---|---|---|---|---|---|---|---|
| Monel K500 | N05500 | 2.4375 | NiCu30Al | – | NA 18 | – | – |
Equivalents are approximate, and few national standards list an exact match for K500. Order to the standard named in your specification.
Aged K500 shafts for seawater pumps and small-craft propellers, combining high fatigue strength with resistance to flowing seawater.
Measurement-while-drilling collars and instrument housings, where K500 stays non-magnetic near survey sensors and keeps its strength under downhole torque and bending loads.
Bolts, studs and nuts for subsea equipment, valves and hull fittings that need more strength than Monel 400 can provide.
Stems, seats, doctor blades and impellers in seawater and chemical duty, where aged K500 resists erosion, galling and wear better than Monel 400.
Cold-drawn and aged wire and bar for springs, scraper blades and gauge components that must keep their spring properties in corrosive media.
Ageing is typically done at about 590–610 °C for several hours, up to 16 hours, followed by slow furnace cooling to around 480 °C and air cooling. The cycle varies with prior cold work, so follow the material standard or purchase specification.
Buy aged bar if the part needs only light machining. Buy solution-annealed bar if heavy machining, forming or welding comes first, then age the finished part to reach full strength.
ASTM B865 covers age-hardenable Monel K500 (UNS N05500). ASTM B164 covers Monel 400 and related solid-solution nickel-copper alloys, which cannot be age hardened.
K500 is listed in NACE MR0175 / ISO 15156 with conditions on heat treatment and maximum hardness. Check the current edition and state the requirement on your order so hardness can be confirmed on the certificate.
K500 is essentially non-magnetic at room temperature and below, which is why it is widely used for drill collars and instrument housings near magnetic sensors.