SS 904L pipe is a super-austenitic stainless steel with 19–23% chromium, 23–28% nickel, 4–5% molybdenum and 1–2% copper, and carbon held to 0.020% maximum. The high nickel keeps the structure fully austenitic and improves resistance to chloride stress corrosion cracking, the molybdenum raises pitting and crevice resistance well above 316L and 317L, and the copper gives the alloy its notable resistance to sulphuric acid across a wide range of concentrations.
Because of its nickel content, UNS N08904 is covered by nickel-alloy standards as well as stainless ones. Seamless pipe and tube are supplied to ASTM B677 / ASME SB677, welded pipe to ASTM B673 and welded tube to ASTM B674. ASTM A312 also lists N08904, so many process specifications accept either A312 or B677 seamless pipe; the chemistry limits differ slightly between the two. The pipe is solution annealed and rapidly cooled, and the very low carbon means welded joints need no post-weld heat treatment to avoid sensitisation.
904L is used where SS 317 / 317L pipe is not resistant enough, particularly in reducing acids. For higher strength in chloride service, duplex steel pipe is an alternative, and for hotter or more aggressive acids, nickel alloys such as Incoloy 825 pipe are considered. For 904L, Metals Fabrica checks whether your specification calls for the B677 or A312 route and can arrange PMI and third-party inspection where the acid service warrants it.
Seamless N08904 pipe and tube to the nickel-alloy standard B677, commonly specified for acid plant lines and exchanger tubing in pressure service.
Seamless or welded 904L ordered to the stainless pipe standard A312, convenient where the piping class already references A312 for all stainless lines.
Welded N08904 pipe for larger diameters and thinner walls, used for acid transfer lines and scrubber piping where seamless pipe would be costly.
Welded N08904 tube sized by outside diameter for heat exchangers and coolers handling seawater, brackish water or acidic process streams.
Small-diameter seamless 904L tube, ordered by outside diameter and wall, for instrumentation, sampling and exchanger bundles in phosphoric and sulphuric acid plants.
| Specification | Details |
|---|---|
| Seamless pipe and tube | ASTM B677 / ASME SB677 UNS N08904 |
| Stainless pipe standard | ASTM A312 / ASME SA312 UNS N08904 |
| Welded pipe and tube | ASTM B673 / ASME SB673 (pipe), ASTM B674 / ASME SB674 (tube) |
| UNS / Werkstoff Nr. | N08904 / 1.4539 |
| Dimension standards | ASME B36.19M, ASME B36.10M |
| Size range | 1/8" NB to 24" NB seamless; up to 48" NB welded |
| Wall thickness | SCH 5S, 10S, 40S, 80S, 160, XXS |
| Heat treatment | Solution annealed and rapidly cooled; pickled |
| Ends and length | Plain, bevelled (ASME B16.25) or threaded; single random, double random or cut length |
| Testing | Hydrostatic or non-destructive electric test per the product standard; pitting test to ASTM G48, ultrasonic and PMI on request |
| Documentation | EN 10204 3.1 mill test certificate; EN 10204 3.2 on request |
State whether B677 or A312 governs the order, as chemistry limits and test requirements differ.
| Standard | UNS | C | Mn | Si | P | S | Cr | Ni | Mo | Cu | N |
|---|---|---|---|---|---|---|---|---|---|---|---|
| ASTM A312 | N08904 | 0.020 | 2.00 | 1.00 | 0.040 | 0.030 | 19.0 – 23.0 | 23.0 – 28.0 | 4.0 – 5.0 | 1.0 – 2.0 | 0.10 |
| ASTM B677 | N08904 | 0.020 | 2.00 | 1.00 | 0.045 | 0.035 | 19.0 – 23.0 | 23.0 – 28.0 | 4.0 – 5.0 | 1.0 – 2.0 | – |
Fe is the balance. Pipe certified to both standards must meet the tighter limit of each.
| Grade | Density | Melting Range | Tensile Strength, min | Yield Strength (0.2% Offset), min | Elongation in 50 mm, min |
|---|---|---|---|---|---|
| 904L (N08904) | 8.00 g/cm³ | 1300 – 1390 °C | 490 MPa (71 ksi) | 215 MPa (31 ksi) | 35% |
Density and melting range are typical values, not specification requirements.
| Grade | UNS | Werkstoff Nr. | EN | JIS | BS | AFNOR | GOST |
|---|---|---|---|---|---|---|---|
| SS 904L | N08904 | 1.4539 | X1NiCrMoCu25-20-5 | SUS 890L | 904S13 | Z2NCDU25-20 | 06ХН28МДТ |
Equivalents are approximate; SUS 890L and 06ХН28МДТ differ from N08904 in several elements. Order to the standard named in your specification.
Acid coolers, dilution and transfer lines, where the copper and molybdenum in 904L resist sulphuric acid at concentrations that attack 316L.
Wet-process phosphoric acid lines and evaporator tubing, where fluorides and chlorides in the acid demand high molybdenum and nickel.
Cooling water tubes and brine lines where 904L resists pitting and chloride stress corrosion cracking better than standard austenitic grades.
Scrubber recirculation piping and spray headers handling acidic, chloride-rich condensate from flue gas cleaning systems, where 317L may not give enough margin against pitting.
Bleach plant equipment and pharmaceutical process lines that handle aggressive chemicals and need a stable austenitic alloy with low carbon.
ASTM B677 / ASME SB677 covers seamless N08904 pipe and tube. ASTM A312 also lists N08904, and welded pipe and tube are covered by ASTM B673 and B674.
904L has much more nickel (23–28%), more molybdenum (4–5%) and added copper. These give far better resistance to sulphuric acid, pitting and chloride stress corrosion cracking than 316L, at a higher cost.
904L performs better than 316L and 317L in seawater and brackish water, but crevice corrosion is still possible in warm, stagnant seawater. Super duplex or 6% molybdenum alloys are often chosen for the most demanding seawater duty.
No. With carbon at 0.020% or less, 904L does not sensitise during welding. Over-alloyed filler metals are usually used so that the weld matches the corrosion resistance of the pipe.
It is a super-austenitic stainless steel, as iron is still the largest element. Its high nickel content is why it is also listed in ASTM B nickel-alloy standards with a UNS N-number.