SS 316 bar (UNS S31600) is an austenitic chromium-nickel stainless steel with 2.00 – 3.00% molybdenum. The molybdenum raises resistance to pitting and crevice corrosion in chlorides, seawater, brines and many process chemicals, which makes 316 the usual bar grade for valve trim, pump shafts and marine hardware where 304 would pit.
The three grades differ only in carbon. 316L (S31603) limits carbon to 0.030% so welded or brazed parts stay free of sensitisation, and it is often dual certified 316/316L. 316H (S31609) holds carbon between 0.04 and 0.10% to give better creep and stress-rupture strength in pressure parts above about 525 °C, such as valve bodies and fittings in steam and hydrocarbon service. ASTM A479 / ASME SA479 is the standard for pressure-retaining bar and also recognises strain-hardened 316 for higher-strength shafts and bolting; ASTM A276 covers general-purpose bar.
Choose 316L for welded parts in corrosive service, 316H for elevated-temperature pressure parts, and annealed or strain-hardened 316 for machined components. For stronger chloride or acid resistance, see SS 317 / 317L bars; for welded parts held at high temperature, see SS 316Ti bars. Metals Fabrica supplies 316, 316L and 316H bar and confirms the carbon grade and condition your specification requires.
Annealed low-carbon round bar, black or peeled, for parts that will be welded into assemblies such as valve bodies, nozzles and fittings in chloride service.
One heat meeting the carbon limit of 316L and the strength minimums of 316, accepted wherever either grade is specified on the drawing or data sheet.
Controlled 0.04 – 0.10% carbon bar to ASTM A479 for pressure parts above about 525 °C, where creep strength governs the allowable stress.
Cold-worked 316 bar with raised yield strength, recognised in ASTM A479, used for pump shafts, bolting and stems that need more strength than annealed bar.
Cold-drawn or centreless-ground 316 and 316L bar to h9 or h11 tolerance for precision shafts, spindles and turned instrument components.
Hexagon bar for compression fittings and nuts, and flat or square bar for marine brackets, keys and fabricated supports in salt-laden environments.
| Specification | Details |
|---|---|
| Bar standards | ASTM A276, ASTM A479 / ASME SA479 Type 316, 316L, 316H |
| UNS | S31600 (316), S31603 (316L), S31609 (316H) |
| Shapes | Round, hexagon, square, flat, rectangular |
| Size range | Round bar 3 mm to 500 mm diameter; hex and square to order |
| Length | 1 m to 6 m random, fixed and cut lengths |
| Condition | Solution annealed; cold finished; strain hardened (316) to ASTM A479 |
| Finish | Black, peeled, turned, bright drawn, centreless ground, polished |
| Tolerance | h9 or h11 for bright bar; k12 or h11 for peeled bar; hot-rolled tolerances per ASTM A484 |
| Testing | Chemical analysis, tensile and hardness tests; IGC test to ASTM A262, ultrasonic testing, PMI and grain size (316H) on request |
| Documentation | EN 10204 3.1 mill test certificate; EN 10204 3.2 with third-party inspection on request |
State the grade, condition and any NACE MR0175 / ISO 15156 hardness requirement in your enquiry.
| Grade | UNS | C | Mn | Si | P | S | Cr | Ni | Mo | N |
|---|---|---|---|---|---|---|---|---|---|---|
| 316 | S31600 | 0.08 | 2.00 | 1.00 | 0.045 | 0.030 | 16.0 – 18.0 | 10.0 – 14.0 | 2.00 – 3.00 | 0.10 |
| 316L | S31603 | 0.030 | 2.00 | 1.00 | 0.045 | 0.030 | 16.0 – 18.0 | 10.0 – 14.0 | 2.00 – 3.00 | 0.10 |
| 316H | S31609 | 0.04 – 0.10 | 2.00 | 1.00 | 0.045 | 0.030 | 16.0 – 18.0 | 10.0 – 14.0 | 2.00 – 3.00 | – |
| Grade | Tensile Strength, min | Yield Strength (0.2% Offset), min | Elongation in 50 mm, min | Reduction of Area, min | Density (typical) | Melting Range (typical) |
|---|---|---|---|---|---|---|
| 316 | 515 MPa (75 ksi) | 205 MPa (30 ksi) | 30% | 40% | 8.00 g/cm³ | 1375 – 1400 °C |
| 316L | 485 MPa (70 ksi) | 170 MPa (25 ksi) | 30% | 40% | 8.00 g/cm³ | 1375 – 1400 °C |
| 316H | 515 MPa (75 ksi) | 205 MPa (30 ksi) | 30% | 40% | 8.00 g/cm³ | 1375 – 1400 °C |
Density and melting range are typical values, not specification requirements. ASTM A276 Condition A hot-finished bar requires 40% elongation and 50% reduction of area; strain-hardened 316 has higher strength minimums that depend on size and level.
| Grade | UNS | Werkstoff Nr. | EN | JIS | BS | AFNOR | GOST |
|---|---|---|---|---|---|---|---|
| SS 316 | S31600 | 1.4401 / 1.4436 | X5CrNiMo17-12-2 | SUS 316 | 316S31 | Z7CND17-11-02 | – |
| SS 316L | S31603 | 1.4404 / 1.4435 | X2CrNiMo17-12-2 | SUS 316L | 316S11 | Z3CND17-11-02 | 03Х17Н14М3 |
| SS 316H | S31609 | 1.4919 | X6CrNiMo17-13-2 | – | 316S51 | – | – |
Equivalents are approximate; 1.4919 is a creep-resisting grade whose limits differ from 316H. Order to the standard named in your specification.
Shackles, shafts, fasteners and deck fittings machined from 316 bar, where molybdenum gives the pitting resistance needed in salt spray and splash zones.
Stems, discs, seats and glands for chemical, water and hydrocarbon valves, using 316L for welded bodies and strain-hardened 316 for stems.
Shafts, sleeves and impeller hubs for seawater, brine and process pumps, often in strain-hardened 316 bar for added fatigue and yield strength.
Agitator shafts, sanitary fittings and machined manifolds in 316L bright bar, chosen for clean surfaces and resistance to chloride-based cleaning agents.
316H bar for fittings, nozzles and valve components in steam, refinery and petrochemical service above 525 °C, where creep strength is required by code.
Machined internals, couplings and fasteners for bleach, sulphite and dilute acid environments that attack 304 bar, using 316L wherever parts are welded.
The grades differ in carbon. 316L has 0.030% maximum carbon for welded parts, 316 allows up to 0.08%, and 316H requires 0.04 – 0.10% carbon for creep strength at high temperature. Chromium, nickel and molybdenum ranges are the same.
316 bar performs well in splash zones, marine atmospheres and moving seawater. In stagnant seawater or tight crevices it can still pit, so duplex or higher-alloy grades are often chosen for fully immersed critical parts.
It is 316 bar cold worked after annealing to raise its yield and tensile strength. ASTM A479 recognises strain-hardened levels whose minimums depend on bar size, and it is used for pump shafts, stems and bolting.
316H is specified for pressure-retaining parts designed for service above about 525 °C. ASME allowable stresses at those temperatures depend on the controlled carbon content, which standard 316L cannot guarantee.
The nearest EN equivalent is 1.4404 (X2CrNiMo17-12-2), supplied as bar to EN 10088-3. 1.4435 has higher molybdenum and nickel. Equivalents are close but not identical, so order to the standard on your drawing.