SS 304 bar (UNS S30400) is the 18% chromium, 8% nickel austenitic stainless steel used for more machined and fabricated stainless parts than any other grade. It resists atmospheric corrosion, fresh water, food acids and most oxidising chemicals, is non-magnetic when annealed, and keeps its toughness at cryogenic temperatures. It cannot be hardened by heat treatment; strength is raised only by cold working.
304L (UNS S30403) limits carbon to 0.030%, which prevents chromium carbide precipitation when bar ends are welded to other components, so welded parts keep their corrosion resistance without re-annealing. Its minimum tensile and yield strengths are slightly lower than 304, so bar is commonly melted and certified as dual 304/304L. Bar for pressure-retaining parts is ordered to ASTM A479 / ASME SA479; general machined parts are often bought to ASTM A276, and cold-finished bar under 12.7 mm carries higher strength minimums in A276.
Choose 304/304L bar for general corrosion service in low-chloride environments. Where chlorides, seawater or reducing acids are present, move to SS 316 / 316L bars. Metals Fabrica supplies 304 and 304L bar in black, peeled and bright conditions and confirms which grade, standard and tolerance your drawing calls for. Matching SS 304 / 304L flanges and sheets and plates are also available.
Hot-rolled or forged rounds, supplied black or peeled, used as stock for shafts, bushes, flanges and turned components in general corrosion service.
Cold-drawn or centreless-ground 304L bar to h9 or h11 tolerance for precision machining, with low carbon for parts that will be welded after machining.
Cold-drawn hexagon bar measured across flats for nuts, unions, couplings and instrument fittings, reducing machining time compared with round stock.
Hot-rolled or cut flat, square and rectangular bar for brackets, supports, frames and wear plates in food, architectural and process equipment.
Bar meeting the 0.030% carbon limit of 304L and the 515 MPa tensile minimum of 304, so a single heat satisfies either grade on the drawing.
Cold-drawn 304 bar with higher strength than annealed bar, covered by ASTM A276 cold-finished minimums or A479 strain-hardened levels for bolting and shafts.
| Specification | Details |
|---|---|
| Bar standards | ASTM A276, ASTM A479 / ASME SA479 Type 304, 304L |
| UNS | S30400 (304), S30403 (304L) |
| Shapes | Round, hexagon, square, flat, rectangular |
| Size range | Round bar 3 mm to 500 mm diameter; hex and square to order |
| Length | 1 m to 6 m random, fixed and cut lengths |
| Condition | Solution annealed; cold finished; strain hardened on request |
| Finish | Black, peeled, turned, bright drawn, centreless ground, polished |
| Tolerance | h9 or h11 for bright bar; k12 or h11 for peeled bar; hot-rolled tolerances per ASTM A484 |
| Testing | Chemical analysis, tensile and hardness tests; IGC test to ASTM A262 Practice E, ultrasonic testing and PMI on request |
| Documentation | EN 10204 3.1 mill test certificate; EN 10204 3.2 with third-party inspection on request |
Confirm the standard, condition, size tolerance and length in your enquiry.
| Grade | UNS | C | Mn | Si | P | S | Cr | Ni | N |
|---|---|---|---|---|---|---|---|---|---|
| 304 | S30400 | 0.08 | 2.00 | 1.00 | 0.045 | 0.030 | 18.0 – 20.0 | 8.0 – 10.5 | 0.10 |
| 304L | S30403 | 0.030 | 2.00 | 1.00 | 0.045 | 0.030 | 18.0 – 20.0 | 8.0 – 12.0 | 0.10 |
| Grade | Tensile Strength, min | Yield Strength (0.2% Offset), min | Elongation in 50 mm, min | Reduction of Area, min | Density (typical) |
|---|---|---|---|---|---|
| 304 | 515 MPa (75 ksi) | 205 MPa (30 ksi) | 30% | 40% | 8.00 g/cm³ |
| 304L | 485 MPa (70 ksi) | 170 MPa (25 ksi) | 30% | 40% | 8.00 g/cm³ |
Density is a typical value, not a specification requirement. Melting range is typically 1400 – 1450 °C.
| Grade / Product | Tensile Strength, min | Yield Strength (0.2% Offset), min | Elongation in 50 mm, min | Reduction of Area, min |
|---|---|---|---|---|
| 304, hot finished | 515 MPa (75 ksi) | 205 MPa (30 ksi) | 40% | 50% |
| 304L, hot finished | 485 MPa (70 ksi) | 170 MPa (25 ksi) | 40% | 50% |
| 304 / 304L, cold finished up to 12.7 mm | 620 MPa (90 ksi) | 310 MPa (45 ksi) | 30% | 40% |
| 304, cold finished over 12.7 mm | 515 MPa (75 ksi) | 205 MPa (30 ksi) | 30% | 40% |
Confirm the condition and size band against the edition of ASTM A276 named in your purchase order.
| Grade | UNS | Werkstoff Nr. | EN | JIS | BS | AFNOR | GOST |
|---|---|---|---|---|---|---|---|
| SS 304 | S30400 | 1.4301 | X5CrNi18-10 | SUS 304 | 304S31 | Z7CN18-09 | 08Х18Н10 |
| SS 304L | S30403 | 1.4306 / 1.4307 | X2CrNi19-11 / X2CrNi18-9 | SUS 304L | 304S11 | Z3CN18-10 | 03Х18Н11 |
Equivalents are close but not identical in every element. EN bar is supplied to EN 10088-3; order to the standard named in your specification.
Shafts, rollers, pins and fittings for processing, filling and packaging lines, where 304L resists cleaning chemicals and food acids without tainting product.
Bolts, studs, nuts and threaded rod made from 304 round and hex bar for general corrosion service in buildings, equipment and utilities.
Stems, spindles and bushes for water, steam condensate and mild chemical service where chloride levels are low enough for 304.
Machined parts for liquid nitrogen, oxygen and LNG equipment, where annealed 304L keeps its impact toughness at very low temperatures.
Handrail posts, balusters, fixings and decorative sections in polished 304 bar for indoor and sheltered outdoor installations away from direct salt spray.
Low-carbon 304L bar machined into internals and fittings for nitric acid and oxidising chemical service, where its chromium content gives good resistance.
304L limits carbon to 0.030% against 0.08% for 304, which protects welded areas from intergranular corrosion. 304L has lower annealed minimums of 485 MPa tensile and 170 MPa yield, compared with 515 MPa and 205 MPa for 304.
Order ASTM A479 / ASME SA479 when the bar becomes a pressure-retaining part of a boiler or pressure vessel, such as a valve body or nozzle. ASTM A276 is suitable for general machined parts. Dual-certified A276/A479 bar covers both.
Annealed 304 bar is essentially non-magnetic. Cold drawing, straightening and heavy machining can create some martensite, so bright bar and machined surfaces may show slight magnetism without loss of corrosion resistance.
No. 304 and 304L are austenitic and do not respond to quench hardening. Strength can be increased only by cold working, for example by cold drawing or strain hardening as recognised in ASTM A276 and A479.
Centreless-ground 304 bright bar is commonly ordered to ISO h9 or h11, while peeled bar is usually supplied to k12 or h11. State the tolerance class and surface finish in the enquiry.