SS 17-7 PH Bar Supplier in Mumbai, India

STAINLESS STEEL BARS
Metals Fabrica supplies 17-7 PH (UNS S17700) stainless bar to ASTM A564 Type 631 and aerospace specifications on enquiry, alongside 17-7 PH strip and wire to ASTM A693 and A313.
Steel bars and rods
OVERVIEW

SS 17-7 PH Bar Overview

17-7 PH (UNS S17700, Type 631) is a semi-austenitic precipitation-hardening stainless steel with about 17% chromium, 7% nickel and 1% aluminium. In the solution-annealed Condition A it is austenitic and formable. A conditioning treatment then transforms it to martensite, and a final ageing step precipitates nickel-aluminium compounds to give high strength. This three-stage route is different from martensitic PH grades such as 17-4 PH, which are martensitic as supplied.

Two standard sequences are used. TH1050 conditions the material at 760 °C, cools it to about 15 °C to form martensite, then ages it at 566 °C. RH950 conditions at 955 °C, refrigerates it at about −73 °C, then ages it at 510 °C for higher strength. ASTM A564 lists Type 631 for bars and shapes, but most 17-7 PH is produced as strip, sheet and spring wire to ASTM A693, ASTM A313 and AMS specifications for springs, washers, bellows and clips. Bar is a limited, mill-order product in a narrow size range.

Choose 17-7 PH where its spring and forming properties are needed in a machined or headed part; for most high-strength machined components, 17-4 PH bar or 15-5 PH bar is more readily available and simpler to heat treat. Metals Fabrica handles 17-7 PH bar enquiries by first confirming the specification, size and minimum quantity with the source mill.

  • Standards: ASTM A564 / ASME SA564 Type 631; strip and plate ASTM A693; spring wire ASTM A313
  • Structure: semi-austenitic; austenitic in Condition A
  • Hardening: conditioning, transformation and ageing (TH1050, RH950)
  • Availability: bar is produced in limited sizes, usually to order
TYPES & VARIANTS

Types of SS 17-7 PH Bar

17-7 PH Bar, Condition A

Solution-annealed austenitic bar supplied for machining, heading or forming, then conditioned and aged by the user to TH1050 or RH950.

17-7 PH TH1050 Condition

Conditioned at 760 °C, transformed on cooling and aged at 566 °C, giving 1170 MPa minimum tensile strength with good toughness.

17-7 PH RH950 Condition

Conditioned at 955 °C, refrigerated at about −73 °C and aged at 510 °C, giving the highest bar strength of 1275 MPa minimum tensile.

17-7 PH Wire and Rod

Small-diameter rod and spring wire to ASTM A313 and AMS specifications, the most common long-product form of 17-7 PH, for springs and clips.

Alternative PH Bar Grades

Where 17-7 PH bar is not available in the required size, 17-4 PH or 15-5 PH bar to ASTM A564 can often meet the strength requirement.

SPECIFICATIONS

SS 17-7 PH Bar Specifications

SpecificationDetails
Bar standardASTM A564 / ASME SA564 Type 631
Related standardsASTM A693 (plate, sheet, strip), ASTM A313 (spring wire), AMS specifications for bar, strip and wire
UNS / Werkstoff Nr.S17700 / 1.4568
ShapesRound bar and wire rod; other shapes subject to availability
Size rangeTo be confirmed per enquiry; bar is produced in limited sizes
LengthRandom and cut lengths to order
ConditionCondition A (solution annealed); TH1050 or RH950 after conditioning and ageing
FinishPeeled, turned, cold drawn, centreless ground
TestingChemical analysis, tensile and hardness in the specified condition; PMI on request
DocumentationEN 10204 3.1 mill test certificate; EN 10204 3.2 with third-party inspection on request

17-7 PH bar is not a widely stocked product. Lead time, minimum quantity and size range are confirmed with each enquiry.

CHEMICAL COMPOSITION

SS 17-7 PH Bar Chemical Composition

Weight %, maximum unless a range is shown, per ASTM A564 Type 631.
GradeUNSCMnSiPSCrNiAl
Type 631 (17-7 PH)S177000.091.001.000.0400.03016.0 – 18.06.50 – 7.750.75 – 1.50
MECHANICAL PROPERTIES

SS 17-7 PH Bar Mechanical Properties

Minimum room-temperature properties for hardened bar per ASTM A564 Type 631.
ConditionTensile Strength, minYield Strength (0.2% Offset), minElongation in 4D, minReduction of Area, minHardness, min
RH9501275 MPa (185 ksi)1030 MPa (150 ksi)6%10%41 HRC
TH10501170 MPa (170 ksi)965 MPa (140 ksi)6%25%38 HRC

Condition A is soft and austenitic, with maximum hardness limits rather than minimum strength. Typical density is 7.81 g/cm³ in Condition A (not a specification requirement).

EQUIVALENT GRADES

SS 17-7 PH Bar Equivalent Grades

GradeUNSWerkstoff Nr.ENJISBSAFNORGOST
17-7 PH (Type 631)S177001.4568X7CrNiAl17-7SUS 631301S81Z9CNA17-0709Х17Н7Ю

Equivalents are approximate and not identical in every element. Order to the standard named in your specification.

APPLICATIONS

SS 17-7 PH Bar Applications

Springs and Spring Components

Coil spring ends, spring seats and machined spring parts that need high strength and fatigue resistance with stainless corrosion resistance.

Aerospace Hardware

Clips, retainers, fasteners and small structural parts formed or machined in Condition A and then hardened to TH1050 or RH950.

Valve and Pressure Instrument Parts

Diaphragm retainers, bellows end fittings and instrument parts where high strength is needed at moderate temperatures up to about 315 °C.

Retaining Rings and Washers

Retaining rings, Belleville washers and lock components that rely on the spring properties and corrosion resistance of hardened 17-7 PH.

WHY METALS FABRICA

Why Choose Metals Fabrica for SS 17-7 PH Bar?

  • Availability checked first: we confirm with the source whether 17-7 PH bar can be produced in your size and quantity before quoting.
  • Specification review: ASTM A564 Type 631 or the AMS specification on your drawing is confirmed, with the delivery condition.
  • Alternatives suggested: where bar is not practical, we can compare 17-4 PH or 13-8 PH bar against your requirements.
  • Documentation: EN 10204 3.1 certificates for 17-7 PH bar, with third-party inspection coordinated when your order requires it.
FAQ

SS 17-7 PH Bar FAQs

Not widely. Most 17-7 PH is produced as strip, sheet and spring wire. Bar to ASTM A564 Type 631 is usually made to order in limited sizes, so size, minimum quantity and lead time must be confirmed for each enquiry.

17-7 PH is semi-austenitic and hardened with aluminium through a conditioning, transformation and ageing sequence. 17-4 PH is martensitic as supplied and hardened with copper by a single ageing step, which makes it simpler to process as bar.

They are two hardening sequences. TH1050 conditions at 760 °C, cools to transform and ages at 566 °C. RH950 conditions at 955 °C, refrigerates at about −73 °C and ages at 510 °C to give higher strength.

ASTM A564 Type 631 covers bars and shapes, ASTM A693 covers plate, sheet and strip, and ASTM A313 covers spring wire. AMS specifications are used for aerospace product forms.

REQUEST A QUOTE

Request a Quote for SS 17-7 PH Bar