15-5 PH bar (UNS S15500, ASTM A564 Type XM-12) is a martensitic precipitation-hardening stainless steel with about 15% chromium, 4.5% nickel and 3.5% copper. It was developed from 17-4 PH with a rebalanced composition: slightly lower chromium and higher nickel keep the structure free of delta ferrite, so the bar has more uniform properties through its cross-section and markedly better transverse ductility and toughness.
Heat treatment follows the same route as 17-4 PH. Bar is solution treated (Condition A) at about 1040 °C, machined, then aged between 482 °C and 621 °C to precipitate copper-rich particles. ASTM A564 sets the same minimum tensile, yield and hardness values for XM-12 as for Type 630 in each H condition. Aerospace bar is normally consumable-electrode remelted (ESR or VAR) and certified to AMS 5659, which adds cleanliness and transverse property requirements that air-melted A564 bar does not carry.
Choose 15-5 PH over 17-4 PH for large sections, forgings and parts loaded across the grain, such as aircraft fittings, actuator housings and valve bodies, where transverse toughness matters. Compare with 17-4 PH bar for general use, or 13-8 PH bar for higher strength. Metals Fabrica supplies 15-5 PH bar and confirms the melting route, condition and specification before quoting.
Solution-treated XM-12 bar supplied for rough and finish machining before ageing, so the user can select the final H condition for the part.
Consumable-electrode vacuum or electroslag remelted bar to AMS 5659 for aircraft structures, with tighter inclusion limits and transverse property testing.
Aged at 552 °C for 1070 MPa minimum tensile with good toughness, a common choice for aerospace fittings, valve stems and high-strength shafts.
Over-aged condition with 930 MPa minimum tensile and improved resistance to stress corrosion cracking for parts in humid or marine environments.
Large-diameter round bar used as forging and ring-rolling stock, where the ferrite-free structure gives uniform properties after forging and ageing.
| Specification | Details |
|---|---|
| Bar standards | ASTM A564 / ASME SA564 Type XM-12; AMS 5659 (consumable-electrode remelted) |
| UNS / Werkstoff Nr. | S15500 / 1.4545 |
| Shapes | Round, hexagon, square, flat |
| Size range | Round bar 3 mm to 500 mm diameter; hex and square to order |
| Length | 1 m to 6 m random, fixed and cut lengths |
| Melting route | Air melted (A564) or ESR / VAR remelted (AMS 5659) |
| Condition | Condition A (solution treated); aged H900 to H1150M |
| Finish | Black, peeled, turned, centreless ground |
| Tolerance | h9 or h11 for ground bar; k12 or h11 for peeled bar |
| Testing | Chemical analysis, tensile and hardness in the specified condition; transverse tensile, macro-etch, ultrasonic testing and PMI on request |
| Documentation | EN 10204 3.1 mill test certificate; EN 10204 3.2 with third-party inspection on request |
State whether AMS 5659 remelted bar is required; air-melted A564 bar does not meet aerospace cleanliness clauses.
| Grade | UNS | C | Mn | Si | P | S | Cr | Ni | Cu | Nb + Ta |
|---|---|---|---|---|---|---|---|---|---|---|
| XM-12 (15-5 PH) | S15500 | 0.07 | 1.00 | 1.00 | 0.040 | 0.030 | 14.0 – 15.5 | 3.5 – 5.5 | 2.5 – 4.5 | 0.15 – 0.45 |
AMS 5659 sets tighter limits on some elements; check the specification named on your order.
| Condition | Tensile Strength, min | Yield Strength (0.2% Offset), min | Elongation in 4D, min | Reduction of Area, min | Hardness, min |
|---|---|---|---|---|---|
| H900 | 1310 MPa (190 ksi) | 1170 MPa (170 ksi) | 10% | 40% | 40 HRC |
| H1025 | 1070 MPa (155 ksi) | 1000 MPa (145 ksi) | 12% | 45% | 35 HRC |
| H1075 | 1000 MPa (145 ksi) | 860 MPa (125 ksi) | 13% | 45% | 32 HRC |
| H1150 | 930 MPa (135 ksi) | 725 MPa (105 ksi) | 16% | 50% | 28 HRC |
| H1150M | 795 MPa (115 ksi) | 515 MPa (75 ksi) | 18% | 55% | 24 HRC |
Longitudinal values. Typical density is 7.80 g/cm³ (not a specification requirement). AMS 5659 sets its own longitudinal and transverse requirements by condition.
| Grade | UNS | Werkstoff Nr. | EN | JIS | BS | AFNOR | GOST |
|---|---|---|---|---|---|---|---|
| 15-5 PH (XM-12) | S15500 | 1.4545 | X5CrNiCu15-5 | – | – | Z7CNU15-05 | – |
Equivalents are approximate; 1.4545 is mainly specified through aerospace EN standards. Order to the standard named in your specification.
Wing and fuselage fittings, brackets and attach lugs machined from AMS 5659 bar, where transverse toughness and stress corrosion resistance are both critical.
Actuator rods, housings, pistons and gear components needing high strength in all directions, aged typically to H1025 or H1075.
High-pressure valve stems, bodies and seats for oil, gas and chemical service where uniform properties through thick sections are required.
Turbine parts, shafts, fasteners and internal components in power plants that need corrosion resistance and strength well above austenitic grades.
Forging stock for rings, flanges and large-diameter shafts, where the ferrite-free structure avoids weak transverse properties after forging.
15-5 PH has lower chromium and higher nickel, which removes delta ferrite from the structure. The result is better transverse ductility and toughness, especially in large sections, while ASTM A564 minimum strengths in each condition are the same.
AMS 5659 is the aerospace material specification for 15-5 PH bars, forgings and rings produced by consumable-electrode remelting. It adds cleanliness and property requirements beyond ASTM A564 and is specified for flight hardware.
H1025 and H1075 are common for aerospace and valve parts because they balance strength and toughness. H900 gives maximum strength, while H1150 and H1150M improve toughness and stress corrosion resistance.
It can be welded in Condition A or an over-aged condition with matching filler, followed by re-solution treatment and ageing for full properties. Welding of aged high-strength parts is generally avoided.