Metals Fabrica supplies 15-5 PH (UNS S15500) stainless bar to ASTM A564 / ASME SA564 Type XM-12 and AMS 5659, in Condition A or aged conditions from H900 to H1150M.
Steel bars and rods
OVERVIEW

SS 15-5 PH Bar Overview

15-5 PH bar (UNS S15500, ASTM A564 Type XM-12) is a martensitic precipitation-hardening stainless steel with about 15% chromium, 4.5% nickel and 3.5% copper. It was developed from 17-4 PH with a rebalanced composition: slightly lower chromium and higher nickel keep the structure free of delta ferrite, so the bar has more uniform properties through its cross-section and markedly better transverse ductility and toughness.

Heat treatment follows the same route as 17-4 PH. Bar is solution treated (Condition A) at about 1040 °C, machined, then aged between 482 °C and 621 °C to precipitate copper-rich particles. ASTM A564 sets the same minimum tensile, yield and hardness values for XM-12 as for Type 630 in each H condition. Aerospace bar is normally consumable-electrode remelted (ESR or VAR) and certified to AMS 5659, which adds cleanliness and transverse property requirements that air-melted A564 bar does not carry.

Choose 15-5 PH over 17-4 PH for large sections, forgings and parts loaded across the grain, such as aircraft fittings, actuator housings and valve bodies, where transverse toughness matters. Compare with 17-4 PH bar for general use, or 13-8 PH bar for higher strength. Metals Fabrica supplies 15-5 PH bar and confirms the melting route, condition and specification before quoting.

  • Standards: ASTM A564 / ASME SA564 XM-12, AMS 5659
  • Structure: martensitic, essentially free of delta ferrite
  • Conditions: A, H900, H925, H1025, H1075, H1100, H1150, H1150M
  • Advantage: better transverse toughness than 17-4 PH
TYPES & VARIANTS

Types of SS 15-5 PH Bar

15-5 PH Bar, Condition A

Solution-treated XM-12 bar supplied for rough and finish machining before ageing, so the user can select the final H condition for the part.

15-5 PH CEVM Bar to AMS 5659

Consumable-electrode vacuum or electroslag remelted bar to AMS 5659 for aircraft structures, with tighter inclusion limits and transverse property testing.

15-5 PH H1025 Bar

Aged at 552 °C for 1070 MPa minimum tensile with good toughness, a common choice for aerospace fittings, valve stems and high-strength shafts.

15-5 PH H1150 Bar

Over-aged condition with 930 MPa minimum tensile and improved resistance to stress corrosion cracking for parts in humid or marine environments.

15-5 PH Forging Stock

Large-diameter round bar used as forging and ring-rolling stock, where the ferrite-free structure gives uniform properties after forging and ageing.

SPECIFICATIONS

SS 15-5 PH Bar Specifications

SpecificationDetails
Bar standardsASTM A564 / ASME SA564 Type XM-12; AMS 5659 (consumable-electrode remelted)
UNS / Werkstoff Nr.S15500 / 1.4545
ShapesRound, hexagon, square, flat
Size rangeRound bar 3 mm to 500 mm diameter; hex and square to order
Length1 m to 6 m random, fixed and cut lengths
Melting routeAir melted (A564) or ESR / VAR remelted (AMS 5659)
ConditionCondition A (solution treated); aged H900 to H1150M
FinishBlack, peeled, turned, centreless ground
Toleranceh9 or h11 for ground bar; k12 or h11 for peeled bar
TestingChemical analysis, tensile and hardness in the specified condition; transverse tensile, macro-etch, ultrasonic testing and PMI on request
DocumentationEN 10204 3.1 mill test certificate; EN 10204 3.2 with third-party inspection on request

State whether AMS 5659 remelted bar is required; air-melted A564 bar does not meet aerospace cleanliness clauses.

CHEMICAL COMPOSITION

SS 15-5 PH Bar Chemical Composition

Weight %, maximum unless a range is shown, per ASTM A564 Type XM-12.
GradeUNSCMnSiPSCrNiCuNb + Ta
XM-12 (15-5 PH)S155000.071.001.000.0400.03014.0 – 15.53.5 – 5.52.5 – 4.50.15 – 0.45

AMS 5659 sets tighter limits on some elements; check the specification named on your order.

MECHANICAL PROPERTIES

SS 15-5 PH Bar Mechanical Properties

Minimum room-temperature properties by condition per ASTM A564 Type XM-12.
ConditionTensile Strength, minYield Strength (0.2% Offset), minElongation in 4D, minReduction of Area, minHardness, min
H9001310 MPa (190 ksi)1170 MPa (170 ksi)10%40%40 HRC
H10251070 MPa (155 ksi)1000 MPa (145 ksi)12%45%35 HRC
H10751000 MPa (145 ksi)860 MPa (125 ksi)13%45%32 HRC
H1150930 MPa (135 ksi)725 MPa (105 ksi)16%50%28 HRC
H1150M795 MPa (115 ksi)515 MPa (75 ksi)18%55%24 HRC

Longitudinal values. Typical density is 7.80 g/cm³ (not a specification requirement). AMS 5659 sets its own longitudinal and transverse requirements by condition.

EQUIVALENT GRADES

SS 15-5 PH Bar Equivalent Grades

GradeUNSWerkstoff Nr.ENJISBSAFNORGOST
15-5 PH (XM-12)S155001.4545X5CrNiCu15-5––Z7CNU15-05–

Equivalents are approximate; 1.4545 is mainly specified through aerospace EN standards. Order to the standard named in your specification.

APPLICATIONS

SS 15-5 PH Bar Applications

Aircraft Structural Fittings

Wing and fuselage fittings, brackets and attach lugs machined from AMS 5659 bar, where transverse toughness and stress corrosion resistance are both critical.

Actuators and Landing Gear Parts

Actuator rods, housings, pistons and gear components needing high strength in all directions, aged typically to H1025 or H1075.

Valve Bodies and Trim

High-pressure valve stems, bodies and seats for oil, gas and chemical service where uniform properties through thick sections are required.

Nuclear and Power Components

Turbine parts, shafts, fasteners and internal components in power plants that need corrosion resistance and strength well above austenitic grades.

Forged Rings and Large Shafts

Forging stock for rings, flanges and large-diameter shafts, where the ferrite-free structure avoids weak transverse properties after forging.

WHY METALS FABRICA

Why Choose Metals Fabrica for SS 15-5 PH Bar?

  • Specification checked: we confirm whether your order needs air-melted ASTM A564 XM-12 or remelted AMS 5659 bar.
  • Condition matched: Condition A for machining or aged bar in the H condition stated on your drawing.
  • Test plan reviewed: longitudinal and transverse tensile, hardness, macro-etch and UT requirements noted before quoting.
  • Grade guidance: help comparing 15-5 PH with 17-4 PH and maraging steel bars for strength and toughness.
  • Documentation: EN 10204 3.1 certificates, with third-party inspection coordinated when required.
FAQ

SS 15-5 PH Bar FAQs

15-5 PH has lower chromium and higher nickel, which removes delta ferrite from the structure. The result is better transverse ductility and toughness, especially in large sections, while ASTM A564 minimum strengths in each condition are the same.

AMS 5659 is the aerospace material specification for 15-5 PH bars, forgings and rings produced by consumable-electrode remelting. It adds cleanliness and property requirements beyond ASTM A564 and is specified for flight hardware.

H1025 and H1075 are common for aerospace and valve parts because they balance strength and toughness. H900 gives maximum strength, while H1150 and H1150M improve toughness and stress corrosion resistance.

It can be welded in Condition A or an over-aged condition with matching filler, followed by re-solution treatment and ageing for full properties. Welding of aged high-strength parts is generally avoided.