13-8 PH bar (UNS S13800, ASTM A564 Type XM-13), often called 13-8 Mo, is a martensitic precipitation-hardening stainless steel with about 12.5% chromium, 8% nickel, 2.2% molybdenum and 1.1% aluminium. Unlike 17-4 PH and 15-5 PH, it is hardened by nickel-aluminium precipitates rather than copper, which gives higher strength with good fracture toughness in both longitudinal and transverse directions.
The alloy is produced by vacuum induction melting followed by vacuum arc remelting, and the composition is held to very low limits for carbon, silicon, phosphorus, sulphur and nitrogen. Bar is solution treated at about 927 °C and cooled below about 16 °C to complete the martensite transformation, then aged between 510 °C (H950) and 621 °C (H1150). In H950 it reaches 1515 MPa minimum tensile strength, which is above the peak strength of the copper-hardened PH grades. Its corrosion resistance is broadly similar to 17-4 PH, and higher ageing temperatures improve resistance to stress corrosion cracking.
Choose 13-8 PH bar for highly stressed aircraft structure, landing gear and actuator parts, and for components where the strength of 17-4 PH is not enough but maraging steel would lack corrosion resistance. Compare with 15-5 PH bar and maraging steel bars. Metals Fabrica supplies 13-8 PH bar to the aerospace or ASTM specification on your order and confirms the condition before quoting.
Solution-treated and cooled bar supplied for machining before ageing, with a small, predictable dimensional change during the final ageing treatment.
Aged at 510 °C or 538 °C for the highest strength levels, 1515 and 1415 MPa minimum tensile, used for highly loaded structural parts.
Intermediate ageing conditions trading some strength for higher toughness and stress corrosion resistance in aircraft fittings and actuator parts.
Over-aged conditions with lower strength and the best toughness and stress corrosion resistance, used for parts in corrosive or humid environments.
VIM and VAR melted bar, forgings and rings to AMS 5629 with the cleanliness, grain flow and testing requirements specified for flight hardware.
| Specification | Details |
|---|---|
| Bar standards | ASTM A564 / ASME SA564 Type XM-13; AMS 5629 |
| UNS / Werkstoff Nr. | S13800 / 1.4534 |
| Shapes | Round, square, flat |
| Size range | Round bar 3 mm to 500 mm diameter; square and flat to order |
| Length | 1 m to 6 m random, fixed and cut lengths |
| Melting route | Vacuum induction melted and vacuum arc remelted (VIM + VAR) |
| Condition | Condition A (solution treated); aged H950, H1000, H1025, H1050, H1100, H1150, H1150M |
| Finish | Black, peeled, turned, centreless ground |
| Testing | Chemical analysis, tensile and hardness in the specified condition; transverse tensile, macro-etch, cleanliness, ultrasonic testing and PMI on request |
| Documentation | EN 10204 3.1 mill test certificate; EN 10204 3.2 with third-party inspection on request |
13-8 PH bar is a specialised aerospace product. Confirm the specification, condition and size in your enquiry.
| Grade | UNS | C | Mn | Si | P | S | Cr | Ni | Mo | Al | N |
|---|---|---|---|---|---|---|---|---|---|---|---|
| XM-13 (13-8 PH) | S13800 | 0.05 | 0.20 | 0.10 | 0.010 | 0.008 | 12.25 – 13.25 | 7.5 – 8.5 | 2.0 – 2.5 | 0.90 – 1.35 | 0.01 |
| Condition | Ageing | Tensile Strength, min | Yield Strength (0.2% Offset), min | Elongation in 4D, min | Reduction of Area, min | Hardness, min |
|---|---|---|---|---|---|---|
| H950 | 510 °C, 4 h | 1515 MPa (220 ksi) | 1415 MPa (205 ksi) | 10% | 45% | 45 HRC |
| H1000 | 538 °C, 4 h | 1415 MPa (205 ksi) | 1310 MPa (190 ksi) | 10% | 50% | 43 HRC |
| H1025 | 552 °C, 4 h | 1275 MPa (185 ksi) | 1205 MPa (175 ksi) | 11% | 50% | 41 HRC |
| H1050 | 566 °C, 4 h | 1205 MPa (175 ksi) | 1140 MPa (165 ksi) | 12% | 50% | 40 HRC |
| H1100 | 593 °C, 4 h | 1030 MPa (150 ksi) | 930 MPa (135 ksi) | 14% | 50% | 34 HRC |
| H1150 | 621 °C, 4 h | 930 MPa (135 ksi) | 620 MPa (90 ksi) | 14% | 50% | 30 HRC |
| H1150M | 760 °C, 2 h + 621 °C, 4 h | 860 MPa (125 ksi) | 585 MPa (85 ksi) | 16% | 55% | 26 HRC |
Longitudinal values. Typical density is 7.76 g/cm³ (not a specification requirement). AMS 5629 sets its own requirements, including transverse properties.
| Grade | UNS | Werkstoff Nr. | EN | JIS | BS | AFNOR | GOST |
|---|---|---|---|---|---|---|---|
| 13-8 PH (XM-13) | S13800 | 1.4534 | X3CrNiMoAl13-8-2 | – | – | – | – |
1.4534 is specified mainly through aerospace EN standards and is an approximate equivalent. Order to the standard named in your specification.
Bulkhead fittings, wing attach parts and flap tracks where very high strength must be combined with transverse toughness and corrosion resistance.
Actuator rods, pistons, pins and landing gear components aged to H1000 or H1025 for high load capacity with good fracture toughness.
High-strength bolts, shear pins and bushings that need more strength than 17-4 PH without the corrosion protection maraging steel requires.
Internal fasteners, control mechanism parts and springs in reactors, where vacuum-melted cleanliness, strength and corrosion resistance are all specified together.
Mould components and tooling parts for corrosive plastics, where a hard, polishable stainless steel with low distortion on ageing is needed.
13-8 PH is hardened by nickel-aluminium rather than copper precipitates and is vacuum melted. It reaches higher strength, 1515 MPa minimum in H950 against 1310 MPa for 17-4 PH in H900, with better transverse toughness.
AMS 5629 is the aerospace material specification for 13-8 PH bars, forgings and rings made by vacuum induction melting and consumable-electrode remelting. It sets chemistry, cleanliness and property requirements for flight hardware.
Its martensite finish temperature is low, so the bar is cooled to about 16 °C or below to complete the transformation before ageing. Incomplete transformation leaves retained austenite and lower strength.
Higher ageing temperatures such as H1025 to H1150 give better resistance to stress corrosion cracking and higher toughness. H950 and H1000 are used where maximum strength is the priority.