ASTM A333 Grade 6 is the most widely specified low-temperature carbon steel pipe, often called LTCS pipe. It is a fine-grained, silicon-killed carbon-manganese steel that must pass a Charpy V-notch impact test at −45 °C (−50 °F). Process plants use it wherever piping can be chilled below the limits allowed for ordinary carbon steel, whether by the process, by depressurisation or by climate.
Chemically, Grade 6 resembles A106 Grade B: carbon 0.30% maximum, manganese 0.29–1.06% and silicon 0.10% minimum. The differences are tighter phosphorus and sulphur limits of 0.025% and mandatory heat treatment, either normalising at 815 °C or higher or a controlled hot-finishing route for seamless pipe, followed by impact testing. Its strength minimums, 415 MPa (60 ksi) tensile and 240 MPa (35 ksi) yield, match A106 Grade B, so many mills certify pipe to both standards.
Compared with Grade 1, Grade 6 is stronger at the same test temperature, which is why it dominates new LTCS piping classes. For colder service down to −100 °C, specify Grade 3. Metals Fabrica can quote LTCS Grade 6 pipe together with A420 WPL6 fittings and A350 LF2 flanges, with impact test results confirmed for every heat.
The standard LTCS line pipe in most process plants, normalised or controlled hot finished and impact tested at −45 °C, available in heavy schedules.
Electric-resistance-welded without filler metal, then heat treated and impact tested, giving an economical LTCS option where welded pipe is accepted.
Pipe meeting the chemistry, strength and impact rules of A333 Grade 6 and A106 Grade B, letting one item serve both cold and normal-temperature piping classes.
LTCS pipe ordered with hardness control for sour-service lines, combining −45 °C toughness with the hydrogen sulphide requirements of the project specification.
Pipe impact tested at a temperature colder than −45 °C or to higher energy values when a project specification sets stricter requirements.
| Specification | Details |
|---|---|
| Standard | ASTM A333/A333M Grade 6 / ASME SA333 Grade 6 (UNS K03006) |
| Dimension standard | ASME B36.10M |
| Size range | 1/8" NB to 36" NB seamless |
| Wall thickness | SCH 10 to SCH 160, STD, XS, XXS |
| Manufacturing type | Seamless; ERW (welded with no filler metal) |
| Heat treatment | Normalised at 815 °C (1500 °F) minimum, normalised and tempered, controlled hot finished (seamless), or quenched and tempered |
| Impact test | Charpy V-notch at −45 °C (−50 °F); full size 18 J average, 14 J single minimum |
| Ends | Plain end, bevelled end (ASME B16.25) |
| Length | Single random, double random, cut length |
| Testing | Tension, flattening, impact; hydrostatic or non-destructive electric test on each length; hardness for sour service on request |
| Documentation | EN 10204 3.1 certificate with heat-treatment and impact results; EN 10204 3.2 on request |
For welded LTCS pipe above the sizes made by ERW, ASTM A671 CC60 / CC65 / CC70 with impact testing is normally specified.
| Grade | UNS | C | Mn | P | S | Si |
|---|---|---|---|---|---|---|
| A333 Grade 6 | K03006 | 0.30 | 0.29 – 1.06 | 0.025 | 0.025 | 0.10 min |
Each 0.01% of carbon below 0.30% allows manganese 0.05% above 1.06%, up to 1.35%. A333 also sets footnote limits on residual and microalloying elements for Grade 6; check the current edition.
| Grade | Density | Tensile Strength, min | Yield Strength, min | Elongation in 50 mm, min (long. / trans.) | Charpy Test Temperature | Impact Energy, min (10 × 10 mm) |
|---|---|---|---|---|---|---|
| A333 Grade 6 | 7.85 g/cm³ | 415 MPa (60 ksi) | 240 MPa (35 ksi) | 30% / 16.5% | −45 °C (−50 °F) | 18 J (13 ft·lbf) average of 3; 14 J (10 ft·lbf) single |
Elongation is the basic minimum for strip and full-section specimens. Sub-size Charpy specimens carry proportionally reduced energy values. Density is typical, not an A333 requirement.
| Grade | UNS | EN / DIN | JIS | BS | GB | IS |
|---|---|---|---|---|---|---|
| A333 Grade 6 | K03006 | P265NL (EN 10216-4) / TTSt 41 N | STPL 380 (JIS G3460) | BS 3603 430 LT50 | 16MnDG (GB/T 18984) | – |
Equivalents are approximate. EN 10216-4, JIS G3460 and GB/T 18984 use their own impact temperatures and energy levels; compare these as well as strength.
Inlet, dehydration and compressor piping in gas plants, where Joule-Thomson cooling during pressure letdown can drop metal temperatures well below zero.
Flare headers and emergency depressurisation lines that cool rapidly as high-pressure gas expands, making −45 °C impact-tested pipe a common design requirement.
Butane and propane transfer, storage and loading lines at terminals and bottling plants, where vaporising LPG chills the pipe wall.
Industrial ammonia refrigeration and fertiliser plant cold lines operating down to about −45 °C, where LTCS is the economical alternative to stainless steel.
Above-ground piping at wellsites, terminals and processing facilities exposed to severe winter ambient temperatures, where ordinary carbon steel would fall below its permitted minimum design temperature.
LTCS means low-temperature carbon steel. In piping, it almost always refers to ASTM A333 Grade 6, which is heat treated and impact tested at −45 °C so it remains tough in cold service.
Usually yes. Grade 6 has the same strength minimums as A106 Grade B, with tighter phosphorus and sulphur limits, heat treatment and impact testing. Many mills supply pipe dual certified to both standards; check that the certificate lists both if you need it.
Grade 6 is Charpy V-notch tested at −45 °C (−50 °F). Full-size specimens must average at least 18 J with no single value below 14 J. Projects can order testing at colder temperatures or higher energies as a supplementary requirement.
The usual companions are ASTM A350 LF2 Class 1 flanges and forged fittings, and ASTM A420 WPL6 butt-weld fittings, which are also impact tested at −45 °C.
A333 allows welded pipe made without filler metal, normally ERW, provided it is heat treated and impact tested. Whether it is acceptable depends on your piping class; some project specifications require seamless pipe for LTCS.