A672 B60 is EFW pipe formed from ASTM A515 Grade 60 plate and welded with filler metal. Its base metal must meet 415–550 MPa tensile strength and 220 MPa minimum yield, the lowest strength level among the A672 B grades.
The defining feature is the plate. A515 is killed with silicon and made to coarse austenitic grain practice, a route intended for intermediate- and higher-temperature service rather than low-temperature toughness. In Grade 60, carbon is limited to 0.24% for plate up to 25 mm and 0.27% up to 50 mm, with manganese at 0.90% maximum. That lean chemistry makes B60 the easiest of the B grades to weld, but its coarse grain gives lower notch toughness than the fine-grain A516 plate used in A672 C60.
B60 is chosen mainly where a plant specification or an existing line already calls for it, typically hot water, low-pressure steam and process lines that never run cold. For new designs needing toughness, the C grades are usually preferred, and for higher pressure in the same family see A672 B70. For B60 pipe, Metals Fabrica checks that A515 plate is acceptable to your design code and that the pipe class and radiography requirement are stated in the enquiry.
No post-weld heat treatment; Class 12 adds a hydrostatic test. Common for thinner-wall hot water and utility lines where the code does not demand stress relief.
Stress relieved after welding and pressure tested, used for thicker B60 walls in sustained hot service where residual seam stress should be reduced.
As-welded pipe with full radiography of the longitudinal seam and a hydrostatic test, for lines where the design code assumes full weld joint efficiency.
Fabrication-ready lengths ordered to match an existing B60 line, so the replacement keeps the original material designation, wall thickness and allowable stress basis.
| Specification | Details |
|---|---|
| Product standard | ASTM A672 Grade B60 |
| Plate material | ASTM A515 Grade 60 (UNS K02401) |
| Classes | 10–13, 20–23, 30–33, 40–43 |
| Dimension standard | ASME B36.10M |
| Size range | 16" OD and larger per ASTM A672 scope; supply up to 100" NB |
| Wall thickness | Up to 75 mm (3 in); SCH 10 to SCH 160, STD, XS, XXS where applicable |
| Manufacturing type | EFW with filler metal, longitudinal seam |
| Heat treatment | Per class: none, stress relieved, normalized, or normalized and tempered |
| Testing | Weld tension and guided-bend tests; radiography and hydrostatic test per class |
| Ends and length | Plain or bevelled (ASME B16.25); random or cut lengths |
| Coating | Black, varnished, 3LPE or FBE on request |
| Documentation | EN 10204 3.1; EN 10204 3.2 with third-party inspection on request |
Confirm the class and wall thickness; B60 is not suitable as a substitute for impact-tested pipe.
| Grade / Plate Thickness | UNS | C | Mn | P | S | Si |
|---|---|---|---|---|---|---|
| B60, t ≤ 25 mm | K02401 | 0.24 | 0.90 | 0.025 | 0.025 | 0.15 – 0.40 |
| B60, 25 < t ≤ 50 mm | K02401 | 0.27 | 0.90 | 0.025 | 0.025 | 0.15 – 0.40 |
| B60, 50 < t ≤ 75 mm | K02401 | 0.29 | 0.90 | 0.025 | 0.025 | 0.15 – 0.40 |
| C60 for comparison, t ≤ 12.5 mm (A516 Gr 60) | K02100 | 0.21 | 0.60 – 0.90 | 0.025 | 0.025 | 0.15 – 0.40 |
The comparison row shows the fine-grain A516 plate used for A672 C60.
| Test | Tensile Strength | Yield Strength, min | Elongation in 200 mm, min | Elongation in 50 mm, min | Density |
|---|---|---|---|---|---|
| B60 base plate | 415 – 550 MPa (60 – 80 ksi) | 220 MPa (32 ksi) | 21% | 25% | 7.85 g/cm³ |
| B60 transverse weld tension | 415 MPa (60 ksi) min | – | – | – | – |
Density is typical. A515 has no mandatory impact requirement; toughness is lower than A516 of the same strength.
| Grade | UNS | EN / DIN | JIS | BS | GB | IS |
|---|---|---|---|---|---|---|
| A672 B60 (A515 Gr 60) | K02401 | P265GH / 1.0425 | SB 410 | – | Q245R | – |
Approximate equivalents by strength. EN P265GH and GB Q245R are fine-grain steels, so they match B60 in strength but not in grain practice.
Large-bore pressurised hot water headers in district heating and industrial plants, operating well above ambient where coarse-grain A515 plate is acceptable.
Steam and condensate return lines at modest pressures, where B60's 220 MPa yield is sufficient and its lean chemistry simplifies field welding.
Like-for-like replacement in older refineries and power plants whose original piping class was written around A672 B60 or A515 Grade 60 plate.
Utility and process lines that always run warm, so the lower notch toughness of coarse-grain steel does not limit the design.
Both have 415–550 MPa tensile and 220 MPa minimum yield strength. B60 uses coarse-grain A515 plate intended for intermediate and higher temperatures, while C60 uses fine-grain A516 plate with lower carbon limits and better notch toughness.
It is not intended for it. Coarse-grain A515 steel has lower impact toughness, so low-temperature lines normally use A671 CC grades or A672 C grades with impact testing.
Under A515 Grade 60, carbon is 0.24% maximum for plate up to 25 mm, 0.27% up to 50 mm and 0.29% up to 100 mm, with manganese limited to 0.90%.
Many existing plants have piping classes built around A515-based pipe, and replacing like with like avoids requalifying the design. New projects more often choose C grades for their fine-grain toughness.