ASTM A672 is the specification for electric-fusion-welded steel pipe, made with filler metal from pressure-vessel quality plate, for high-pressure service at moderate temperatures. It is the large-diameter counterpart of seamless process pipe such as ASTM A106 Grade B, used where line sizes of 16 inch OD and above make plate-formed pipe the practical route.
A672 grade names encode the plate. The letter identifies the plate specification and the number gives its minimum tensile strength in ksi. The B grades are made from ASTM A515, a silicon-killed steel melted to coarse-grain practice and intended for intermediate and higher temperatures. The C grades are made from ASTM A516, a fine-grain steel for moderate and lower temperatures with better notch toughness. Other A672 grades use A285, A537 and carbon-molybdenum A204 plate. Plate pages: A515 Grade 70 and A516 Grade 70.
Each order also states a class, written as two digits. The first records what heat treatment the finished pipe received after welding, and the second records whether the seam was radiographed, the pipe pressure tested, or both. Where the same plate is needed for low-temperature duty, ASTM A671 applies instead. Metals Fabrica helps decide between B grades on A515 plate and C grades on A516 plate, and confirms the class designation that governs heat treatment and testing before quoting.
A672 pipe is defined by grade and class. Read the class as two digits: first the post-weld heat treatment (1 none, 2 stress relieved, 3 normalized, 4 normalized and tempered), then the inspection (0 none, 1 radiography, 2 pressure test, 3 both).
Made from ASTM A515 coarse-grain plate with carbon up to 0.35% in the strongest grade. Traditionally specified for hot process and steam-related lines at intermediate temperatures.
Made from ASTM A516 fine-grain plate. Preferred in most current piping specifications because the fine grain gives better toughness and more predictable weld properties.
The finished pipe receives no heat treatment after the seam is welded. Suitable where wall thickness stays below the code threshold for mandatory post-weld heat treatment.
Heat treated below the critical range after welding to relax seam residual stresses. Widely used for thicker walls and for services prone to stress-related cracking.
Normalized, or normalized and tempered, after welding to restore uniform structure across plate, weld and heat-affected zone; usually specified for heavy walls.
Lower-strength A grades on A285 plate, higher-strength D grades on A537, and L grades on carbon-molybdenum A204 plate for somewhat higher temperatures.
| Specification | Details |
|---|---|
| Product standard | ASTM A672 (electric-fusion-welded steel pipe for high-pressure service at moderate temperatures) |
| Grades | B60, B65, B70 (ASTM A515 plate); C60, C65, C70 (ASTM A516 plate); other grades on enquiry |
| Classes | 10–13, 20–23, 30–33, 40–43 |
| Dimension standard | ASME B36.10M |
| Size range | 16" OD and larger per ASTM A672 scope; supply up to 100" NB |
| Wall thickness | Up to 75 mm (3 in); SCH 10 to SCH 160, STD, XS, XXS where applicable |
| Manufacturing type | EFW with filler metal, longitudinal seam (LSAW-type) |
| Heat treatment | As welded, stress relieved, normalized, or normalized and tempered per class |
| Testing | Transverse weld tension and guided-bend tests; radiography and hydrostatic test per class |
| Ends and length | Plain or bevelled (ASME B16.25); single random, double random, cut length |
| Coating | Black, varnished, 3LPE or FBE on request |
| Documentation | EN 10204 3.1; EN 10204 3.2 with third-party inspection on request |
State the grade, class, OD, wall thickness and length in your enquiry.
| Grade | UNS (plate) | C, t ≤ 25 mm | C, 25 < t ≤ 50 mm | C, 50 < t ≤ 100 mm | Mn | P | S | Si |
|---|---|---|---|---|---|---|---|---|
| B60 | K02401 | 0.24 | 0.27 | 0.29 | 0.90 | 0.025 | 0.025 | 0.15 – 0.40 |
| B65 | K02800 | 0.28 | 0.31 | 0.33 | 0.90 | 0.025 | 0.025 | 0.15 – 0.40 |
| B70 | K03101 | 0.31 | 0.33 | 0.35 | 1.20 | 0.025 | 0.025 | 0.15 – 0.40 |
| Grade | UNS (plate) | C, t ≤ 12.5 mm | C, 12.5 < t ≤ 50 mm | C, 50 < t ≤ 100 mm | Mn | P | S | Si |
|---|---|---|---|---|---|---|---|---|
| C60 | K02100 | 0.21 | 0.23 | 0.25 | 0.60 – 0.90 (t ≤ 12.5 mm); 0.85 – 1.20 (t > 12.5 mm) | 0.025 | 0.025 | 0.15 – 0.40 |
| C65 | K02403 | 0.24 | 0.26 | 0.28 | 0.85 – 1.20 | 0.025 | 0.025 | 0.15 – 0.40 |
| C70 | K02700 | 0.27 | 0.28 | 0.30 | 0.85 – 1.20 | 0.025 | 0.025 | 0.15 – 0.40 |
A672 pipe walls are limited to 75 mm, so only the bands up to 100 mm are shown.
| Grade | Plate | Tensile Strength | Yield Strength, min | Elongation in 200 mm, min | Elongation in 50 mm, min |
|---|---|---|---|---|---|
| B60 | A515 Gr 60 | 415 – 550 MPa (60 – 80 ksi) | 220 MPa (32 ksi) | 21% | 25% |
| B65 | A515 Gr 65 | 450 – 585 MPa (65 – 85 ksi) | 240 MPa (35 ksi) | 19% | 23% |
| B70 | A515 Gr 70 | 485 – 620 MPa (70 – 90 ksi) | 260 MPa (38 ksi) | 17% | 21% |
| C60 | A516 Gr 60 | 415 – 550 MPa (60 – 80 ksi) | 220 MPa (32 ksi) | 21% | 25% |
| C65 | A516 Gr 65 | 450 – 585 MPa (65 – 85 ksi) | 240 MPa (35 ksi) | 19% | 23% |
| C70 | A516 Gr 70 | 485 – 620 MPa (70 – 90 ksi) | 260 MPa (38 ksi) | 17% | 21% |
B and C grades of the same number share tensile limits; they differ in chemistry, grain practice and toughness. Typical density of carbon steel is 7.85 g/cm³.
| Grade | UNS | EN / DIN | JIS | BS | GB | IS |
|---|---|---|---|---|---|---|
| B60 (A515 Gr 60) | K02401 | P265GH / 1.0425 | SB 410 | – | Q245R | – |
| B65 (A515 Gr 65) | K02800 | P295GH / 1.0481 | SB 450 | – | – | – |
| B70 (A515 Gr 70) | K03101 | P355GH / 1.0473 | SB 480 | – | Q345R | – |
| C60 (A516 Gr 60) | K02100 | P265GH / 1.0425 | SGV 410 | BS 1501-224-430 | Q245R | – |
| C65 (A516 Gr 65) | K02403 | P295GH / 1.0481 | SGV 450 | BS 1501-224-460 | – | – |
| C70 (A516 Gr 70) | K02700 | P355GH / 1.0473 | SGV 480 | BS 1501-224-490 | Q345R | – |
Approximate equivalents of the plate steels only. EN and GB pressure-vessel steels are fine-grain and do not reproduce the coarse-grain practice of A515.
Large-bore cooling and circulating water lines between condensers and cooling towers, where diameter and pressure make plate-formed C-grade pipe the economical choice.
Hydrocarbon process and transfer piping at moderate temperatures, in C70 for most new work and in B grades where an existing specification calls for them.
Distribution headers in industrial plants operating at intermediate temperatures, the duty the coarse-grain A515-based B grades were originally developed for.
Raw water, process water and firewater trunk mains of 16 inch and above where seamless pipe is not available and EFW gives controlled wall thickness.
Feed, product and utility headers in petrochemical complexes, with stress-relieved classes specified for thick walls and services sensitive to residual stress.
B grades are made from ASTM A515, a coarse-grain steel intended for intermediate and higher temperatures. C grades are made from ASTM A516, a fine-grain steel with better notch toughness for moderate and lower temperatures. Tensile limits are the same for the same number, but chemistry and toughness differ.
C70 means A516 Grade 70 plate with a 70 ksi minimum tensile strength. In CL32 the 3 means the pipe was normalized after welding and the 2 means it was pressure tested without radiography.
A672 does not set a temperature limit. The design code, such as ASME B31.3 or B31.1, sets allowable stresses by temperature, and long-term service of carbon steel above about 425 °C is restricted because of graphitisation.
No. A672 pipe is always electric-fusion-welded from plate with filler metal, usually with a longitudinal submerged arc seam. For seamless carbon steel pipe, specify ASTM A106 or A53 Type S.
C70 is the most widely used because A516 Grade 70 plate is readily produced and combines good strength with fine-grain toughness. B grades are mainly found in older or specific plant specifications.