ASTM A333 Grade 1 is a plain carbon-manganese pipe steel for low-temperature service. Like every A333 grade, it must pass a Charpy V-notch impact test at a set temperature, for Grade 1 −45 °C (−50 °F), which proves the pipe will not fail by brittle fracture when cold. ASME SA333 Grade 1 is the boiler-and-pressure-vessel code version.
Grade 1 has the lowest strength of the A333 carbon steel grades: 380 MPa (55 ksi) tensile and 205 MPa (30 ksi) yield minimum, with 35% longitudinal elongation. Its chemistry limits carbon to 0.30% and manganese to 0.40–1.06%, with phosphorus and sulphur held at 0.025% each, but, unlike A333 Grade 6, it has no silicon minimum. Toughness comes from heat treatment: the pipe is normalised, normalised and tempered, or, if seamless, finished from a controlled hot-working temperature.
Because Grade 6 offers the same −45 °C test with higher strength, most new projects specify Grade 6, and Grade 1 is chosen mainly where existing designs, thin-wall calculations or bending needs favour its lower strength and greater ductility. Pipe may be seamless or welded without filler metal. For colder duty, A333 Grade 3 is tested at −100 °C. Metals Fabrica checks that the A333 Grade 1 test certificate reports Charpy results at the temperature your piping class specifies, which may be colder than the standard value.
Seamless pipe normalised or finished from a controlled hot-working temperature, then Charpy tested at −45 °C, for cold process lines that exclude weld seams.
Electric-resistance-welded pipe made without filler metal, heat treated and impact tested, offering an economical low-temperature option in small and medium sizes.
Pipe normalised above 815 °C and then tempered, a route mills use to refine grain size and secure consistent impact energy through the wall.
Light schedules where Grade 1's lower strength and higher elongation suit cold bending and forming, and where the design does not need Grade 6 strength.
| Specification | Details |
|---|---|
| Standard | ASTM A333/A333M Grade 1 / ASME SA333 Grade 1 (UNS K03008) |
| Dimension standard | ASME B36.10M |
| Size range | 1/8" NB to 36" NB seamless |
| Wall thickness | SCH 10 to SCH 160, STD, XS, XXS |
| Manufacturing type | Seamless; welded with no filler metal (ERW) |
| Heat treatment | Normalised at 815 °C (1500 °F) minimum, or normalised and tempered; seamless may be controlled hot finished |
| Impact test | Charpy V-notch at −45 °C (−50 °F); full size 18 J average, 14 J single minimum |
| Ends | Plain end, bevelled end (ASME B16.25) |
| Length | Single random, double random, cut length |
| Testing | Tension, flattening, impact; hydrostatic or non-destructive electric test on each length |
| Documentation | EN 10204 3.1 certificate with impact results; EN 10204 3.2 on request |
Very thin walls may be too thin for even the smallest Charpy specimen; A333 then waives or adjusts impact testing. Confirm size and wall in your enquiry.
| Grade | UNS | C | Mn | P | S | Si |
|---|---|---|---|---|---|---|
| A333 Grade 1 | K03008 | 0.30 | 0.40 – 1.06 | 0.025 | 0.025 | – |
For each 0.01% reduction in carbon below 0.30%, manganese may increase by 0.05% above 1.06%, to a maximum of 1.35%.
| Grade | Density | Tensile Strength, min | Yield Strength, min | Elongation in 50 mm, min (long. / trans.) | Charpy Test Temperature | Impact Energy, min (10 × 10 mm) |
|---|---|---|---|---|---|---|
| A333 Grade 1 | 7.85 g/cm³ | 380 MPa (55 ksi) | 205 MPa (30 ksi) | 35% / 25% | −45 °C (−50 °F) | 18 J (13 ft·lbf) average of 3; 14 J (10 ft·lbf) single |
Elongation is the basic minimum for strip and full-section specimens. Lower absorbed-energy values apply to sub-size Charpy specimens. Density is typical, not an A333 requirement.
| Grade | UNS | EN / DIN | JIS | BS | GB | IS |
|---|---|---|---|---|---|---|
| A333 Grade 1 | K03008 | P215NL (EN 10216-4) / TTSt 35 N | STPL 380 (JIS G3460) | – | – | – |
Equivalents are approximate. Impact test temperature and energy differ between standards, so compare these values, not only the grade name.
Brine, glycol and refrigerant lines in industrial cold stores and process chillers, where pipe must stay ductile at design temperatures well below zero.
Outdoor air, gas and water lines in regions where winter metal temperatures fall below the limits allowed for non-impact-tested carbon steel pipe.
Piping downstream of pressure-reducing valves and blowdown lines, where gas expansion cools the pipe wall sharply during operation or emergency venting.
Maintenance and revamp work on plants originally designed with Grade 1, keeping the same material and strength basis as the original piping class.
Both are Charpy tested at −45 °C. Grade 6 requires 0.10% minimum silicon and has higher strength, 415 MPa tensile and 240 MPa yield, against 380 MPa and 205 MPa for Grade 1. Grade 6 is the more common choice for new work.
With full-size 10 × 10 mm Charpy specimens, the average of three specimens must be at least 18 J (13 ft·lbf) and no single specimen below 14 J (10 ft·lbf). Proportionally lower values apply to sub-size specimens.
No. A333 permits seamless pipe and welded pipe made without filler metal, which in practice means electric-resistance welding. Large-diameter low-temperature welded pipe is normally ordered to ASTM A671.
Normalising refines the grain structure, which is what gives carbon steel its toughness at low temperature. The standard requires every A333 Grade 1 pipe to be treated to control its microstructure before impact testing.