ASTM A283 covers carbon steel plates of structural quality in four strength levels, Grades A, B, C and D. Grade C is the most commonly ordered: it requires 380–515 MPa tensile strength and 205 MPa (30 ksi) minimum yield, which places it between mild Grades A and B and the slightly stronger Grade D. It is an economical plate for lightly stressed welded construction.
The chemistry is simple: carbon up to 0.24%, manganese up to 0.90% and phosphorus and sulphur limited to 0.030%. Plate up to 40 mm may have up to 0.40% silicon; heavier plate must be silicon-killed with 0.15–0.40% Si. Copper of 0.20% minimum can be specified for weathering resistance. The plate is supplied as-rolled. Its yield strength is about 18% lower than ASTM A36, and unlike pressure-vessel A285 Grade C it is ordered to the structural tolerances of ASTM A6.
Engineers select A283 Grade C mainly for atmospheric storage tank shells and bottoms under API 650 within its thickness limit, and for non-critical structures where formability and cost matter more than strength. Metals Fabrica supplies A283 Grade C plate, sheet and coil and checks the tank code limits and test needs on each enquiry.
Rectangular plate cut to course width and length for welded atmospheric storage tank shells, ordered within the thickness limit of the tank code.
Thinner plate and sheet for lapped tank bottoms, sketch plates and cone or dome roof plates, cut to the tank layout drawing.
Coil for slitting and cutting to length, used where high volumes of light-gauge parts are formed or pressed.
Plate ordered with 0.20% minimum copper to improve resistance to atmospheric corrosion on unpainted or intermittently painted structures.
The strongest grade in A283, with 230 MPa yield and 415–550 MPa tensile, for designs that need a little more strength than Grade C.
| Specification | Details |
|---|---|
| Standard | ASTM A283 / A283M Grade C (also Grades A, B, D) |
| UNS | K02401 |
| General requirements | ASTM A6 / A6M |
| Thickness | Sheet 0.3 – 6 mm; plate 6 – 150 mm and above |
| Width | 1000, 1219, 1500, 2000, 2500 mm and to order |
| Length | 2000, 2500, 3000, 6000 mm; coils and cut to size |
| Delivery condition | As-rolled |
| Surface finish | Hot rolled black, shot blasted and primed |
| Forms | Plate, sheet, coil, slit strip, cut blanks |
| Testing | One tension test per heat and thickness per ASTM A6; ultrasonic testing on request |
| Documentation | EN 10204 3.1 mill test certificate; EN 10204 3.2 on request |
Tank codes limit the thickness at which A283 Grade C may be used. Confirm the code and shell thickness in your enquiry.
| Grade | Plate thickness | C | Mn | P | S | Si | Cu (when specified) |
|---|---|---|---|---|---|---|---|
| Grade C | ≤ 40 mm | 0.24 | 0.90 | 0.030 | 0.030 | 0.40 | 0.20 min |
| Grade C | > 40 mm | 0.24 | 0.90 | 0.030 | 0.030 | 0.15 – 0.40 | 0.20 min |
| Grade | Tensile Strength | Yield Strength, min | Elongation in 200 mm, min | Elongation in 50 mm, min |
|---|---|---|---|---|
| Grade A | 310 – 415 MPa (45 – 60 ksi) | 165 MPa (24 ksi) | 27% | 30% |
| Grade B | 345 – 450 MPa (50 – 65 ksi) | 185 MPa (27 ksi) | 25% | 28% |
| Grade C | 380 – 515 MPa (55 – 75 ksi) | 205 MPa (30 ksi) | 22% | 25% |
| Grade D | 415 – 550 MPa (60 – 80 ksi) | 230 MPa (33 ksi) | 20% | 23% |
Density about 7.85 g/cm³ (typical, not a requirement).
| Grade | UNS | EN | JIS | GB | IS |
|---|---|---|---|---|---|
| ASTM A283 Grade C | K02401 | S235JR (EN 10025-2) | SS400 | Q235A | IS 2062 E250 A |
Equivalents are approximate; most listed grades have higher minimum yield than A283 Grade C. Substitution needs designer approval.
Shell, bottom and roof plate for API 650 tanks storing water, fuel oil and other products at near-atmospheric pressure, within the code thickness limit.
Bulk-solids containers in cement, grain and mining plants, where good formability and economy outweigh the need for high strength.
Brackets, covers, guards, trench plates and secondary steelwork carrying modest loads, where the lower yield of Grade C is acceptable to the designer.
Rolled and welded sheet for ventilation ducting, flue ducts and stacks operating near ambient temperature in industrial plants and utilities.
Clarifier walls, launders and process tanks in municipal and industrial water plants, usually coated or lined to protect the carbon steel from the water.
Both are structural carbon steel plates to ASTM A6, but A36 has a higher minimum yield of 250 MPa against 205 MPa for A283 Grade C. A283 Grade C has a slightly lower tensile range and is chosen mainly for tanks and lightly loaded parts.
Yes. API 650 lists A283 Grade C for tank shells, bottoms and roofs, subject to a maximum plate thickness given in the code. Thicker shell courses are normally made from A516 or A573 plate.
They have the same tensile range and yield minimum, but A285 is a pressure-vessel plate ordered to ASTM A20, with phosphorus and sulphur limited to 0.025% and a carbon limit of 0.28%. A283 is structural plate to ASTM A6.
Yes. With carbon at 0.24% maximum and manganese at 0.90% maximum it welds readily with standard processes. Preheat is rarely needed for normal thicknesses but should follow the fabrication code.