ASTM A285 covers carbon steel plates of low and intermediate tensile strength for fusion-welded pressure vessels. It has three grades, A, B and C, and Grade C is the strongest, with 380–515 MPa tensile strength and 205 MPa minimum yield. The standard is limited to plate up to 50 mm (2 in) thick, and ASME adopts it as SA285 for pressure parts under Section VIII.
Grade C allows carbon up to 0.28% and manganese up to 0.90%, with phosphorus and sulphur held to 0.025%. Silicon is not specified, so the steel need not be fully killed, which is one reason A285 is an economical vessel plate. Plates are normally supplied as-rolled and may be ordered normalised or stress relieved. As a pressure-vessel grade it follows ASTM A20, so Charpy tests, ultrasonic examination and simulated post-weld heat treatment can be added as supplementary requirements.
A285 Grade C suits low-pressure vessels, air receivers and tanks where design stresses are modest. For higher allowable stress or better notch toughness, A516 Grade 60 or Grade 70 is normally preferred. Metals Fabrica supplies A285 Grade C plate and checks the thickness, heat-treatment condition and supplementary tests against your vessel specification.
The standard delivery condition under ASTM A285, suitable for most low-pressure vessels and tanks where no impact testing is specified.
Plate heated above the critical range and air cooled for a finer, more uniform structure, ordered when the vessel design or impact tests call for it.
Plate certified to ASME SA285 for vessels stamped under ASME Section VIII, with marking and certificate traceable to the heat.
Test coupons given a simulated post-weld heat treatment before tensile testing, so certified properties reflect the fabricated vessel.
Circles and blanks cut from plate for dished ends, manway covers and reinforcing pads, sized to suit the forming allowance of the head maker.
| Specification | Details |
|---|---|
| Standard | ASTM A285 / A285M Grade C; ASME SA285 Grade C |
| UNS | K02801 |
| General requirements | ASTM A20 / A20M (pressure-vessel plate) |
| Thickness | Sheet 0.3 – 6 mm; plate 6 – 50 mm (standard limit) |
| Width | 1000, 1219, 1500, 2000, 2500 mm and to order |
| Length | 2000, 2500, 3000, 6000 mm; coils and cut to size |
| Delivery condition | As-rolled; normalised, stress relieved or both on request |
| Surface finish | Hot rolled black, shot blasted and primed |
| Forms | Plate, sheet, coil, cut blanks, circles |
| Testing | Tension test per A20; Charpy V-notch, ultrasonic (A435 / A578) and simulated PWHT as A20 supplementary requirements |
| Documentation | EN 10204 3.1 mill test certificate; EN 10204 3.2 with third-party inspection on request |
The existing page listed plate to 150 mm, but ASTM A285 covers plate only up to 50 mm. Thicker vessel plate is normally A516.
| Grade | UNS | C | Mn | P | S |
|---|---|---|---|---|---|
| Grade A | K01700 | 0.17 | 0.90 | 0.025 | 0.025 |
| Grade B | K02200 | 0.22 | 0.90 | 0.025 | 0.025 |
| Grade C | K02801 | 0.28 | 0.90 | 0.025 | 0.025 |
Silicon is not specified. Limits on unspecified residual elements (Cu, Ni, Cr, Mo, V, Nb) follow ASTM A20.
| Grade | Tensile Strength | Yield Strength, min | Elongation in 200 mm, min | Elongation in 50 mm, min |
|---|---|---|---|---|
| Grade A | 310 – 450 MPa (45 – 65 ksi) | 165 MPa (24 ksi) | 27% | 30% |
| Grade B | 345 – 485 MPa (50 – 70 ksi) | 185 MPa (27 ksi) | 25% | 28% |
| Grade C | 380 – 515 MPa (55 – 75 ksi) | 205 MPa (30 ksi) | 23% | 27% |
Density about 7.85 g/cm³ (typical, not a requirement).
| Grade | UNS | EN | JIS | GB | IS |
|---|---|---|---|---|---|
| ASTM A285 Grade C | K02801 | P235GH / P265GH (EN 10028-2) | – | Q245R | – |
Equivalents are approximate. EN 10028-2 grades are fine-grain and include impact requirements that A285 does not. Confirm with the vessel designer.
Low-pressure air and gas receivers where design pressure and temperature are moderate and the economy of A285 is an advantage.
Settling tanks, knock-out drums and vessels in chemical and water plants, designed to ASME Section VIII within the 50 mm limit.
Shell and bottom plate for welded storage tanks where the tank code permits A285 Grade C at the required thickness.
Non-critical boiler parts, casings and flue ducts where the purchaser specifies pressure-vessel quality plate rather than structural plate.
Formed heads, manway necks and covers made from the same A285 Grade C plate as the shell, keeping one material specification throughout the vessel.
ASTM A285 covers plates up to 50 mm (2 in) thick. For thicker pressure-vessel plate, A516 or A515 is specified.
A516 Grade 60 is fine-grain, silicon-killed steel with higher strength (415–550 MPa tensile, 220 MPa yield), better notch toughness and thickness up to 200 mm and beyond. A285 Grade C is a lower-strength, economical plate limited to 50 mm.
No. It is normally delivered as-rolled. Normalising or stress relieving can be ordered, and is common when impact tests are required.
It has no impact requirement in the base standard. If the design minimum metal temperature requires toughness, specify Charpy testing under ASTM A20 or select normalised A516 instead.
Approximate equivalents include EN 10028-2 P235GH or P265GH and Chinese Q245R. These grades differ in chemistry and test requirements, so substitution needs the designer’s approval.