A515 Grade 70 is the top strength level of ASTM A515, the standard for carbon-silicon pressure vessel plate in intermediate- and higher-temperature service. It requires 485–620 MPa tensile strength and 260 MPa (38 ksi) minimum yield, so a vessel designed in Grade 70 can use thinner walls than one in Grade 60. ASME lists it as SA515 Grade 70 for boilers and pressure vessels.
The extra strength comes from more carbon and manganese: carbon is 0.31% maximum up to 25 mm and up to 0.35% in plate over 50 mm, with manganese allowed to 1.20% against 0.90% for A515 Grade 60. The steel is killed and made to coarse-grain practice. Plate over 50 mm must be normalised; thinner plate is normally as-rolled. The higher carbon raises the carbon equivalent, so welding procedures usually call for preheat on thicker sections and stress relief as the code requires.
Choose A515 Grade 70 for drums, shells and heads that run hot and need higher allowable stress. If the vessel must also be tough at ambient or low temperatures, A516 Grade 70 gives the same tensile range in fine-grain steel. Metals Fabrica supplies A515 Grade 70 plate and reviews thickness, heat treatment and code marking with every enquiry.
Heavy plate for steam and mud drums, normalised above 50 mm and often ordered with ultrasonic examination to ASTM A578.
Plate up to 50 mm supplied as-rolled for shells and heads where the design does not specify heat treatment.
Plate ordered both normalised and stress relieved, giving stable properties for heavy hot-formed heads and thick nozzle sections in high-temperature boiler work.
Tensile coupons heat treated to simulate the vessel's post-weld heat treatment, so the certificate reflects strength after fabrication.
Thick discs and blanks cut from Grade 70 plate for exchanger tube sheets, blind covers and reinforcing rings that are later machined and drilled.
| Specification | Details |
|---|---|
| Standard | ASTM A515 / A515M Grade 70; ASME SA515 Grade 70 |
| UNS | K03101 |
| General requirements | ASTM A20 / A20M |
| Thickness | Sheet 0.3 – 6 mm; plate 6 – 150 mm and above |
| Width | 1000, 1219, 1500, 2000, 2500 mm and to order |
| Length | 2000, 2500, 3000, 6000 mm; cut to size |
| Steelmaking | Killed, coarse austenitic grain size practice |
| Delivery condition | As-rolled up to 50 mm; normalised over 50 mm; normalised and stress relieved on request |
| Surface finish | Hot rolled black, shot blasted and primed |
| Testing | Tension test per A20; ultrasonic (A435 / A578), simulated PWHT, Charpy V-notch and carbon-equivalent limit as supplementary requirements |
| Documentation | EN 10204 3.1 mill test certificate; EN 10204 3.2 on request |
State the design temperature and code so the right heat treatment and tests are quoted.
| Plate thickness | C | Mn | P | S | Si |
|---|---|---|---|---|---|
| ≤ 25 mm | 0.31 | 1.20 | 0.025 | 0.025 | 0.15 – 0.40 |
| > 25 to 50 mm | 0.33 | 1.20 | 0.025 | 0.025 | 0.15 – 0.40 |
| > 50 mm | 0.35 | 1.20 | 0.025 | 0.025 | 0.15 – 0.40 |
Residual-element limits and product analysis tolerances follow ASTM A20.
| Grade | Tensile Strength | Yield Strength, min | Elongation in 200 mm, min | Elongation in 50 mm, min |
|---|---|---|---|---|
| Grade 70 | 485 – 620 MPa (70 – 90 ksi) | 260 MPa (38 ksi) | 17% | 21% |
Elevated-temperature allowable stresses are in ASME Section II Part D. Density about 7.85 g/cm³ (typical, not a requirement).
| Grade | UNS | EN | JIS | GB | IS |
|---|---|---|---|---|---|
| ASTM A515 Grade 70 | K03101 | P355GH (EN 10028-2) | SB480 (JIS G3103) | Q345R | – |
Equivalents are approximate. P355GH and Q345R are fine-grain steels with different chemistry and impact rules; confirm with the designer.
Steam drums, water-wall headers and boiler shells where the higher allowable stress of Grade 70 reduces drum wall thickness.
Hot-service carbon steel vessels operating well above ambient, within the temperature range where carbon steel is still permitted.
Shells and drums of waste-heat boilers and heat-recovery steam generators handling hot flue gas and steam at elevated temperature and pressure.
Plate formed into ASTM A672 B70 welded pipe for steam and hot process lines larger than seamless sizes.
Shells, channels and tube sheets in exchangers handling hot hydrocarbons or steam, where Grade 70 strength reduces wall thickness over Grade 60.
ASTM A515 Grade 70 requires 485–620 MPa (70–90 ksi) tensile strength and 260 MPa (38 ksi) minimum yield. Elongation must be at least 21% in 50 mm or 17% in 200 mm.
Grade 70 has higher carbon (up to 0.35%) and manganese (up to 1.20%), giving about 70 MPa more tensile strength and 40 MPa more yield. It is harder to weld and usually needs preheat on thick sections.
Yes, mainly for elevated-temperature equipment such as boiler drums. Many designers now prefer A516 Grade 70 for general vessels because fine-grain steel gives better toughness at the same strength.
Normalising is mandatory for plate thicker than 50 mm. Thinner plate may be as-rolled unless the purchaser specifies normalising or stress relieving.
ASTM A672 Grade B70 and ASTM A671 Grade CB70 electric-fusion-welded pipe use A515 Grade 70 plate. The pipe class sets heat treatment and radiography.