A516 Grade 65 sits between Grades 60 and 70 in the ASTM A516 family of fine-grain carbon steel pressure vessel plates. It requires 450–585 MPa (65–85 ksi) tensile strength and 240 MPa (35 ksi) minimum yield. That gives designers roughly 9% more yield than Grade 60 while keeping carbon lower than in Grade 70, a useful compromise when both wall thickness and weldability matter.
Grade 65 is killed, fine-grain steel. Its carbon limit is 0.24% up to 12.5 mm, 0.26% to 50 mm, 0.28% to 100 mm and 0.29% above, and unlike Grade 60 its manganese range of 0.85–1.20% applies at every thickness. Silicon is held at 0.15–0.40% and phosphorus and sulphur at 0.025% each. As with all A516 grades, plate thicker than 40 mm must be normalised, and thinner plate is normalised when impact tests are ordered unless agreed otherwise.
Grade 65 is often written into storage tank and vessel specifications where a plate stronger than Grade 60 is needed but Grade 70’s higher carbon is not wanted, for example on thick shells that must be welded with minimal preheat. Metals Fabrica supplies A516 Grade 65 plate and checks thickness band, normalising, Charpy and certificate requirements before quoting.
Plate normalised for uniform fine-grain structure, compulsory above 40 mm and common for impact-tested orders below that thickness.
Charpy V-notch tested to ASTM A20 at the temperature set by the vessel's minimum design metal temperature and plate thickness under the design code.
Coupons heat treated to simulate post-weld stress relief so tensile and impact results represent the finished vessel rather than the plate as delivered.
Plate examined ultrasonically to ASTM A435 or A578 to confirm freedom from laminations before nozzle welding, cutting or forming into heads.
Plates cut and bevelled to shell course dimensions, or supplied as circles for heads and tube sheets, to reduce cutting at the fabrication shop.
| Specification | Details |
|---|---|
| Standard | ASTM A516 / A516M Grade 65; ASME SA516 Grade 65 |
| UNS | K02403 |
| General requirements | ASTM A20 / A20M |
| Thickness | Sheet 0.3 – 6 mm; plate 6 – 150 mm and above |
| Width | 1000, 1219, 1500, 2000, 2500 mm and to order |
| Length | 2000, 2500, 3000, 6000 mm; coils and cut to size |
| Steelmaking | Killed, fine austenitic grain size practice |
| Delivery condition | As-rolled up to 40 mm; normalised over 40 mm; normalised and stress relieved on request |
| Surface finish | Hot rolled black, shot blasted and primed |
| Testing | Tension test per A20; Charpy V-notch, ultrasonic (A435 / A578), simulated PWHT and carbon-equivalent limit on request |
| Documentation | EN 10204 3.1 mill test certificate; EN 10204 3.2 on request |
Confirm thickness, heat treatment, impact temperature and ultrasonic level in your enquiry.
| Plate thickness | C | Mn | P | S | Si |
|---|---|---|---|---|---|
| ≤ 12.5 mm | 0.24 | 0.85 – 1.20 | 0.025 | 0.025 | 0.15 – 0.40 |
| > 12.5 to 50 mm | 0.26 | 0.85 – 1.20 | 0.025 | 0.025 | 0.15 – 0.40 |
| > 50 to 100 mm | 0.28 | 0.85 – 1.20 | 0.025 | 0.025 | 0.15 – 0.40 |
| > 100 mm | 0.29 | 0.85 – 1.20 | 0.025 | 0.025 | 0.15 – 0.40 |
Product analysis tolerances and residual-element limits are given in ASTM A20.
| Grade | Tensile Strength | Yield Strength, min | Elongation in 200 mm, min | Elongation in 50 mm, min |
|---|---|---|---|---|
| Grade 65 | 450 – 585 MPa (65 – 85 ksi) | 240 MPa (35 ksi) | 19% | 23% |
Density about 7.85 g/cm³ (typical, not a requirement).
| Grade | UNS | EN | JIS | GB | IS |
|---|---|---|---|---|---|
| ASTM A516 Grade 65 | K02403 | P295GH (EN 10028-2) | SGV450 (JIS G3118) | Q345R | – |
Equivalents are approximate and differ in yield, chemistry and impact rules. Confirm suitability with the designer.
Two- and three-phase separators and slug catchers where Grade 65 trims wall thickness compared with Grade 60 without Grade 70's carbon level.
Shell plate for API 650 tanks where design stress calls for more strength than A283 or A285 grades provide.
Shells, channels and covers for exchangers operating from below ambient up to moderate temperatures, with Charpy testing where the design requires it.
Small bullets and storage cylinders where normalised, impact-tested plate is specified for ambient operation and the low temperatures reached during rapid depressurisation.
Plate formed and fusion welded into A671 CC65 and A672 C65 pipe for large-diameter process, fire-water and cooling-water lines.
The minimum yield strength is 240 MPa (35 ksi), with tensile strength between 450 and 585 MPa (65–85 ksi). Elongation must be at least 23% in 50 mm.
Grade 65 is the middle grade: 240 MPa yield against 220 MPa for Grade 60 and 260 MPa for Grade 70. Its carbon limits are also in between, so it balances strength and weldability.
No. Grade 70 has a higher minimum strength, so Grade 65 cannot replace it without redesign. Grade 70 plate can sometimes replace Grade 65 if the designer accepts its higher carbon and strength.
Normalising is required for plate over 40 mm and for thinner plate ordered with impact tests, unless the purchaser agrees to as-rolled impact-tested plate.