ASTM A515 covers carbon-silicon steel plates for intermediate- and higher-temperature service in welded boilers and pressure vessels. Grade 60 is the lowest-strength grade of the standard, with 415–550 MPa tensile strength and 220 MPa (32 ksi) minimum yield, chosen where formability and weldability are valued over maximum allowable stress. ASME adopts it as SA515 Grade 60.
A515 steel is silicon-killed and made to coarse austenitic grain size practice, which gives good creep and elevated-temperature strength but lower notch toughness than fine-grained steel. Carbon is controlled by thickness, from 0.24% in plate up to 25 mm to 0.31% above 100 mm, with manganese limited to 0.90% and silicon held at 0.15–0.40%. Plate up to 50 mm is normally supplied as-rolled; plate over 50 mm must be normalised. The higher-strength A515 Grade 70 uses more carbon and manganese for 485 MPa minimum tensile.
Specify A515 Grade 60 for steam drums, headers and hot process vessels that never see low metal temperatures. For ambient or sub-zero service, fine-grain A516 Grade 60 has the same tensile range with better toughness. Metals Fabrica supplies A515 Grade 60 plate and confirms the thickness band, normalising and any supplementary tests before quoting.
Plate up to 50 mm thick in the as-rolled condition permitted by the standard, for drums and shells where no heat treatment is specified.
Mandatory for plate over 50 mm and available for thinner plate, giving a more uniform structure through heavy boiler drum sections.
Plate certified to ASME SA515 for boilers and vessels built under ASME Sections I and VIII, with heat-traceable marking.
Test coupons receive a simulated post-weld heat treatment so certified properties represent the vessel after stress relief, as many boiler codes expect.
Circles and segments cut from A515 plate for hot-formed dished ends, tube sheets and nozzle reinforcement pads on boilers and drums.
| Specification | Details |
|---|---|
| Standard | ASTM A515 / A515M Grade 60; ASME SA515 Grade 60 |
| UNS | K02401 |
| General requirements | ASTM A20 / A20M |
| Thickness | Sheet 0.3 – 6 mm; plate 6 – 150 mm and above |
| Width | 1000, 1219, 1500, 2000, 2500 mm and to order |
| Length | 2000, 2500, 3000, 6000 mm; cut to size |
| Steelmaking | Killed, coarse austenitic grain size practice |
| Delivery condition | As-rolled up to 50 mm; normalised over 50 mm; normalised or stress relieved on request |
| Surface finish | Hot rolled black, shot blasted and primed |
| Testing | Tension test per A20; ultrasonic (A435 / A578), simulated PWHT and Charpy V-notch as supplementary requirements |
| Documentation | EN 10204 3.1 mill test certificate; EN 10204 3.2 with third-party inspection on request |
Confirm thickness, heat treatment and any ASME code edition in your enquiry.
| Plate thickness | C | Mn | P | S | Si |
|---|---|---|---|---|---|
| ≤ 25 mm | 0.24 | 0.90 | 0.025 | 0.025 | 0.15 – 0.40 |
| > 25 to 50 mm | 0.27 | 0.90 | 0.025 | 0.025 | 0.15 – 0.40 |
| > 50 to 100 mm | 0.29 | 0.90 | 0.025 | 0.025 | 0.15 – 0.40 |
| > 100 mm | 0.31 | 0.90 | 0.025 | 0.025 | 0.15 – 0.40 |
Product analysis tolerances and residual-element limits follow ASTM A20.
| Grade | Tensile Strength | Yield Strength, min | Elongation in 200 mm, min | Elongation in 50 mm, min |
|---|---|---|---|---|
| Grade 60 | 415 – 550 MPa (60 – 80 ksi) | 220 MPa (32 ksi) | 21% | 25% |
Allowable stresses at temperature are given in ASME Section II Part D. Density about 7.85 g/cm³ (typical, not a requirement).
| Grade | UNS | EN | JIS | GB | IS |
|---|---|---|---|---|---|
| ASTM A515 Grade 60 | K02401 | P265GH (EN 10028-2) | SB410 (JIS G3103) | Q245R | – |
Equivalents are approximate. P265GH and Q245R are fine-grain steels with impact requirements; JIS SB410 is the closest boiler-plate match.
Boiler drums and headers in industrial and utility boilers, where coarse-grain A515 gives reliable strength at elevated metal temperatures.
Reactors, columns and heaters in refineries and chemical plants that operate continuously above ambient temperature, where low-temperature toughness is not a design requirement.
Shells and channels for exchangers running hot on both sides, where the design does not call for low-temperature impact toughness or HIC resistance.
Plate formed and fusion welded into ASTM A672 B60 pipe for hot process and steam lines in large diameters.
Pressure shells and storage sections in boiler feedwater systems operating at moderate pressure and elevated temperature in power and process plants.
Both have 415–550 MPa tensile and 220 MPa yield. A515 is made to coarse-grain practice for intermediate- and higher-temperature service, while A516 is made to fine-grain practice for moderate- and lower-temperature service and has better notch toughness.
ASTM A515 requires normalising for plates over 50 mm (2 in) thick. Thinner plate is normally as-rolled but may be ordered normalised or stress relieved.
Thicker plate cools more slowly and needs more carbon to reach the specified strength. A515 Grade 60 allows 0.24% carbon up to 25 mm, rising to 0.31% above 100 mm.
It is not intended for low-temperature service because coarse-grain steel has lower impact toughness. Where the minimum design metal temperature is low, normalised A516 with Charpy testing is the usual choice.